欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

奧氏體不銹鋼的焊接特點:焊接過程中彈塑性應力應變很大,但冷裂紋很少。焊接接頭無淬火硬化區(qū),無晶粒粗化,因此焊縫抗拉強度高。

The main problems of austenitic stainless steel welding are: large welding deformation; because of its grain boundary characteristics and sensitivity to some trace impurities (s, P), it is easy to produce hot cracks.

Five major welding problems and treatment measures of austenitic stainless steel

The formation of chromium carbide reduces the intergranular corrosion resistance of welded joints

Intergranular corrosion: according to the theory of poor chromium, when the weld and heat affected zone are heated to 450 ~ 850 ℃ sensitization temperature zone, chromium carbide precipitates on the grain boundary, resulting in poor chromium grain boundary, which is not enough to resist corrosion. Zero

(1) The following measures can be adopted to limit the intergranular corrosion of weld and the corrosion of sensitized temperature zone on the target material

a. In order to avoid the formation of Cr23C6, stabilizing elements such as Ti and Nb were added to the base metal to reduce the carbon content in the base metal and weld.

b. The dual phase structure of austenite and a small amount of ferrite is formed in the weld. When there is a certain amount of ferrite in the weld, the grain size can be refined, the grain area can be increased, and the amount of chromium carbide precipitation per unit area of grain boundary can be reduced.

Cr23C6 is preferentially formed in ferrite instead of poor chromium at austenite grain boundary; ferrite between austenite can prevent corrosion from diffusing into interior along grain boundary.

c. Control the residence time in the sensitization temperature range. Adjust the welding thermal cycle to shorten the residence time of 600-1000 ℃ as much as possible. The welding method with high energy density (such as plasma argon arc welding) can be selected. The welding line energy is smaller. Argon gas is applied to the back of the weld or copper pad is used to increase the cooling rate of the welded joint. The number of arc striking and arc stopping is reduced to avoid repeated heating. The contact surface between multi-layer welding and corrosive medium is as last as possible Welding, etc.

d. After welding, solid solution treatment or stabilization annealing (850-900 ℃) should be carried out after heat preservation and air cooling to fully precipitate carbide and accelerate chromium diffusion.

(2) For this reason, the following preventive measures can be taken:

Due to the strong diffusion ability of carbon, it will segregate in the grain boundary and form supersaturation state during cooling, while Ti and Nb will remain in the crystal due to the low diffusion ability. When the welded joint is reheated in the sensitized temperature range, the supersaturated carbon will precipitate in the form of Cr23C6.

a. Reduce carbon content. For stainless steel containing stabilizing elements, the carbon content should not exceed 0.06%.

b. Adopt reasonable welding process. In order to reduce the residence time of overheated zone at high temperature, a smaller welding line energy should be selected to avoid “medium temperature sensitization” effect in the welding process.

In case of double side welding, the weld contacting with corrosive medium should be welded last (this is the reason why internal welding of large diameter thick wall welded pipe is carried out after external welding). If it cannot be implemented, the welding specification and weld shape should be adjusted to avoid the overheated area contacting with corrosive medium from being sensitized again.

c. Post weld heat treatment. After welding, solid solution or stabilization treatment shall be carried out.

Why do You Having Problems Frequently when Welding Stainless Steel? 2

Stress corrosion cracking

The following measures can be taken to prevent the occurrence of stress corrosion cracking:

a. Correct selection of materials and reasonable adjustment of weld composition. High purity chromium nickel austenitic stainless steel, high silicon chromium nickel austenitic stainless steel, ferrite austenite stainless steel and high chromium ferrite stainless steel have good stress corrosion resistance. When the weld metal is austenitic ferrite dual phase steel, the stress corrosion resistance is good.

b. Eliminate or reduce the residual stress. The surface residual stress was reduced by polishing, shot peening and hammering.

c. Reasonable structural design. In order to avoid large stress concentration.

Why do You Having Problems Frequently when Welding Stainless Steel? 3

Welding hot crack (weld crystallization crack, HAZ liquefaction crack)

The hot crack sensitivity mainly depends on the chemical composition, microstructure and properties of the material. Ni is easy to form low melting point compounds or eutectic with impurities such as s and P. segregation of boron and silicon will promote hot cracking.

It is easy to form coarse columnar crystal structure with strong directivity, which is conducive to the segregation of harmful impurities and elements, thus promoting the formation of continuous intergranular liquid film and improving the sensitivity of hot cracking. If the welding is heated unevenly, it is easy to form large tensile stress and promote the generation of welding hot cracks.

Preventive measures:

a. The contents of harmful impurities s and P should be strictly controlled.

b. Adjust the structure of weld metal. The δ phase in the weld can refine the grain size, eliminate the directionality of single-phase austenite, reduce the segregation of harmful impurities in the grain boundary, and the δ phase can dissolve more s and P, reduce the interface energy and form the liquid film between grains.

c. Adjust the composition of weld metal alloy. The sensitivity to hot cracking can be reduced by adding Mn, C, N and trace elements such as cerium, pickaxe and tantalum in single phase austenitic steel.

d. Process measures. In order to prevent the formation of coarse columnar grains, the small heat input and small cross-section weld bead should be used.

For example, 25-20 austenitic steel is prone to liquefying cracks. By strictly limiting the impurity content and grain size of the base metal, adopting high energy density welding method, small line energy and increasing the cooling rate of the joint, etc.

Why do You Having Problems Frequently when Welding Stainless Steel? 4

Embrittlement of welded joint

The plasticity of welded joint should be guaranteed for hot strength steel to prevent high temperature embrittlement; low temperature steel should have good low temperature toughness to prevent brittle fracture of welded joint at low temperature.

Welding deformation is large

Due to the low thermal conductivity and large expansion coefficient, the welding deformation is large, so the fixture can be used to prevent deformation. Selection of welding methods and welding materials for austenitic stainless steel: austenitic stainless steel can be welded by TIG, MIG, paw and saw.

The welding current of austenitic stainless steel is small because of its low melting point, small thermal conductivity and high resistance coefficient. Narrow weld and narrow pass should be used to reduce high temperature residence time, prevent carbide precipitation, reduce weld shrinkage stress and reduce hot crack sensitivity.

The composition of welding material, especially Cr and Ni, is higher than that of base metal. The welding material containing a small amount of ferrite (4-12%) is used to ensure good crack resistance (cold cracking, hot cracking and stress corrosion cracking) of the weld.

When ferrite phase is not allowed or impossible to exist in the weld, the welding material containing Mo, Mn and other alloy elements should be selected.

C, s, P, Si and Nb in welding materials should be as low as possible. NB may cause solidification cracks in pure austenite weld, but a small amount of ferrite in the weld can be effectively avoided.

Nb containing welding materials are usually used for welding structures which need to be stabilized or stress relieved after welding. When submerged arc welding is used to weld medium plate, the burning loss of Cr and Ni can be supplemented by the transition of alloy elements in flux and welding wire;

Due to the deep penetration, attention should be paid to prevent the formation of hot cracks in the central zone of the weld and the reduction of corrosion resistance in the heat affected zone. Attention should be paid to the selection of thinner welding wire and smaller welding line energy. The welding wire should be low in Si, s and P.

The ferrite content in weld of heat-resistant stainless steel should not be more than 5%. For austenitic stainless steel with more than 20% Cr and Ni, high Mn (6-8%) welding wire and alkaline or neutral flux should be selected to prevent Si addition to weld and improve its crack resistance.

The special flux for austenitic stainless steel increases little Si, which can transfer alloy to the weld and compensate the burning loss of alloy elements to meet the requirements of weld performance and chemical composition.

Why do You Having Problems Frequently when Welding Stainless Steel? 5
黄色av网站在线免费观看-亚洲欧美精品偷拍tv| 91大神国内精品免费网站-亚洲免费电影一区二区| 亚洲国产视频不卡一区-激情欧美视频一区二区| 俄罗斯胖老太太黄色特级片-国产精品黑丝美腿美臀| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 国产一区二区三区四区五区麻豆-欧美一级在线视频播放| 国产老熟女激情小视频-成人一区二区人妻不卡视频| 亚洲永久免费在线观看-亚洲欧美导航一区二区导航| 午夜日韩精品在线视频-亚洲网老鸭窝男人的天堂| 免费看黄色污污的网站-欧美一区二区三区爽爽| 午夜福利1区2区3区-午夜洗澡免费视频网站| 中文字幕社区电影成人-欧美精美视频一区二区三区| 中文字幕精品一区二区日本99-青青国产成人久久91网| 可以免费看污污视频的网站-日韩欧美不卡视频在线观看| 国产欧美一区二区三区嗯嗯-欧美一区二区日本国产激情| 国产一区二区无套内射-国内精品久久久久久久齐pp| 亚洲av成人一区国产精品网-国产偷_久久一级精品a免费| 中文字幕日韩精品不卡一区二区-成人av在线观看一区二区| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 丝袜高跟熟女视频国产-熟女少妇亚洲一区二区| 午夜日韩精品在线视频-亚洲网老鸭窝男人的天堂| 日韩精品人妻系列一区-亚洲女同性一区二区三区| 99热在线精品免费6-av一区二区在线观看| 国产黄片在现免费观看-色老板最新在线播放一区二区三区| 亚洲另类熟女国产精品-懂色一区二区三区在线播放| 女主播啪啪大秀免费观看-精品99午夜福利影院| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 久久网站中文字幕精品-三级精品久久中文字幕| 国产av一区二区三区日韩接吻-av网址在线播放网站| 日本少妇激情一区二区-亚洲自偷自拍熟女另类蜜臀| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 国模自慰一区二区三区-日韩一级黄色片天天看| 久色高清精品在线国产-国产精品视频一区三区四区| 极品人妻av在线播放-久久精品视频一区二区三区| 人妻互换精品一区二区-夜夜爽一区二区三区视频| 久久精品人妻一区二区三区极品-久久99热这里只有精品免费| hd在线观看一区二区-免费一区二区三区毛片在线| 国产美女裸露无遮挡双奶网站-国产精品色午夜视频免费看| 91大神国内精品免费网站-亚洲免费电影一区二区| 国产成人精品免费视频大全办公室-亚洲欧美日本综合在线| 欧美日本亚一级二级三区久久精品-日韩欧美一区二区久久婷婷|