欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

Low-pressure hot isostatic pressing (HIP) is a new sintering process developed in Western developed countries in the 1980s, which combines vacuum sintering and hot isostatic pressing in a single device to complete the process in one step. We have utilized low-pressure hot isostatic pressing technology to manufacture recycled mining carbide, which effectively improves the mechanical and physical properties of the alloys, resulting in a virtually pore-free microstructure and excellent rock drilling performance on-site.

Hot Isostatic Pressing

Experimental Method

Recycled WC powder with a Fisher particle size of 3.00~10.00 μm and normal WC powder with a Fisher particle size of 10.00~18.00 μm were mixed with Co powder or Ni powder with a loose packing density of 0.5~0.7g/cm3 to prepare mixtures of grades YJ1, YJ2, N309, etc. The mixtures were shaped, degummed, and then sintered in a domestically produced horizontal vacuum furnace and a low-pressure hot isostatic pressing furnace manufactured by a German specialized equipment company. The low-pressure hot isostatic pressing process is as follows: loading → vacuum pumping → heating → maintaining sintering temperature → charging argon and pressurizing → maintaining pressure and temperature → cooling and depressurizing → unloading. Electron microscopy was used for metallographic analysis, and the linear shrinkage and shrinkage rate of the samples during the sintering process were measured by the low-pressure hot isostatic pressing sintering furnace to analyze the densification process. The test alloys were made into D43×22 straight horseshoe bits for calibration tests in mining operations.

Experimental Results

Comparison of Properties

Between Low-Pressure Hot Isostatic Pressing Treatment of Recycled Material and Vacuum Sintering Treatment of Normal Material. The two types of tungsten carbide powders, recycled and normal, were processed using the same manufacturing process, undergoing vacuum sintering and low-pressure hot isostatic pressing treatment, respectively. The results are listed in Table 1.

What's Low-Pressure Hot Isostatic Pressing of Recycled Mining Carbide? 2

As can be seen from Table 1, the porosity of the alloy treated with low-pressure hot isostatic pressing using recycled WC powder is even lower than that of the normal alloy, and its performance has been significantly improved, with an increase in the transverse rupture strength value; moreover, the elimination of type B pores ranging from 10 to 25 μm indicates the intrinsic relationship between the reduction in porosity and the increase in transverse rupture strength, while also confirming the capability of low-pressure hot isostatic pressing sintering to eliminate pores in recycled alloys.

Low-Pressure Hot Isostatic Pressing Alloy Linear Shrinkage Test

The linear shrinkage and shrinkage rate of the samples during the sintering process in the low-pressure hot isostatic pressing furnace were measured as shown in the attached figure. The alloy undergoes two stages: vacuum sintering and hot isostatic pressing. The macroscopic pores are eliminated during the vacuum sintering stage, and the microscopic pores are eliminated during the hot isostatic pressing stage to achieve the final densification level.

Comparison of On-site Rock Drilling Effects

The two types of tungsten carbide?powders, recycled and normal, were made into alloys of grades YJ1, YJ2, N309, etc., and calibration tests were conducted at the Taolin Lead-Zinc Mine. The results are listed in Table 2.

What's Low-Pressure Hot Isostatic Pressing of Recycled Mining Carbide? 3

The rock drilling calibration indicates that high-quality mining carbide?can be produced from recycled WC powder through low-pressure hot isostatic pressing treatment, and their performance is comparable to that of mining carbide?made from normal tungsten carbide.

What's Low-Pressure Hot Isostatic Pressing of Recycled Mining Carbide? 4

Result Analysis

Process Characteristics of Low-Pressure Hot Isostatic Pressing for Eliminating Pores in Recycled carbide

The densification of carbide?primarily occurs during sintering, where the plastic flow of the binder phase and the rearrangement of WC grains are driven by surface tension. However, under atmospheric or vacuum sintering, a certain amount of porosity always remains after shrinkage densification is complete; this is because when pores are sealed, the stress inside the pores reaches equilibrium with the surface tension of the pores. Additionally, due to the mixed composition of recycled materials and the presence of more harmful impurities, large pores and voids are easily formed during vacuum sintering, leading to issues such as low alloy density, low fracture strength, significant hardness variations, and severe contamination of the alloy. Applying a certain pressure can promote further flow of the binder phase and rearrangement of WC grains, thereby greatly reducing or even completely eliminating these pores or voids.

Study on the Densification Mechanism of Low-Pressure Hot Isostatic Pressing

The change curve of the linear shrinkage rate of recycled carbide?samples during low-pressure hot isostatic pressing sintering is shown in the attached figure. There are three peaks on the shrinkage rate curve: Peak A appears at a sintering temperature of 1200°C, which is solid-phase sintering. Due to the low yield point of the binder phase, plastic flow occurs under a small external force. The flow of the binder metal changes the contact situation between powder particles, causing the carbide?particles to move and come closer together. Peak B appears during the liquid-phase sintering process at 1340°C, where WC particle rearrangement, solution precipitation, and skeleton formation result in significant shrinkage of the sintered body, and macroscopic pores are eliminated during the vacuum sintering process of low-pressure hot isostatic pressing. Peak C appears at the beginning of the pressurization stage, where the rise in pressure eliminates the micro-pores in the product. However, with the extension of the pressure maintenance time, no new shrinkage peak appears in the product.

 

??züm

(1) The physical and mechanical properties of the recycled alloy treated by low-pressure hot isostatic pressing are superior to those of alloys manufactured by conventional processes, with a significant reduction in porosity and the elimination of type B pores.

(2) The recycled alloy treated by low-pressure hot isostatic pressing does not fall short of normal alloys in on-site rock drilling tests, and its wear resistance is even improved.

(3) The mechanism by which low-pressure hot isostatic pressing improves the performance of the alloy is mainly the elimination of large-sized pores and the reduction in porosity.

Bir cevap yaz?n

E-posta hesab?n?z yay?mlanmayacak. Gerekli alanlar * ile i?aretlenmi?lerdir

国产在线观看高清精品-四季av一区二区三区中文字幕| 色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 国产精品电影在线一区-亚洲国产大片一区二区官网| 久久高清超碰av热热久久-国产高清不卡免费视频| 99在线观看精品视频免费-国产极品一区二区三区四区| 99久热精品免费观看四虎-亚洲天堂精品视频在线| 性色国产成人久久久精品二区三区-偷窥中国美女洗澡视频| 青青操视频在线观看国产-欧美成人乱码在线观看| 中文字幕偷拍亚洲九色-亚洲视频不卡一区二区天堂| 黄色91av免费在线观看-欧美黄片一级在线观看| 亚洲精品在线观看一二三区-在线观看国产中文字幕视频| 国产av剧情护士麻豆-三级国产精品欧美在线观看| 一区二区三区女同性恋-熟妇高潮一区二区高清网络视频| 久久精品亚洲国产av久-国产精品视频一区二区免费| 一区二区三区国产高清mm-美女张开腿让帅哥桶爽| 欧美精品一区二区不卡-精品国产一区二区三区香蕉网址| 欧美日韩精品人妻在线-在线播放中文字幕一区| 国产精品熟女视频一区二区-国产日韩精品欧美一区喷水| 人妻日韩精品中文字幕图片-麻豆极度性感诱人在线露脸| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 青青操大香蕉在线播放-国产亚洲欧美精品在线观看| 白嫩美女娇喘呻吟高潮-久久一区二区三区日产精品| 交换朋友的妻子中文字幕-日本美女8x8x8x8| av一区免费在线观看-中文字幕日韩国产精品视频| 久久免费观看归女高潮特黄-黄色av一本二本在线观看| 亚洲欧美一区二区中文-台湾中文综合网妹子网| 中文字幕人妻少妇第一页-隔壁的女孩在线看中文字幕| 熟女熟妇伦51788-国产av在线播放一区二区三区| 国产欧美日韩中文字幕在线-国产伊人一区二区三区四区| 亚洲精品一区网站在线观看-黄页视频免费观看网站| 亚洲愉拍自拍欧美精品app-亚洲一区不卡在线视频| 国产人妻人伦精品日本-国产98超碰人人做人人爱| 亚洲区欧美区在线视频-亚洲碰碰人人AV熟女天堂| 国产aa视频一区二区三区-国产精品久久久久久久毛片动漫| 免费午夜福利在线观看-黄色日本黄色日本韩国黄色| 小12萝自慰喷水亚洲网站-chinese偷拍一区二区三区| 白嫩美女娇喘呻吟高潮-久久一区二区三区日产精品| 日韩高清在线观看一区二区-美产av在线免费观看| 性都花花世界亚洲综合-日韩av一区二区三区| 精品一区二区三区av在线-欧美黑人巨大精品一区二区| 亚洲av综合av一区东京热-黄页免费视频网站在线观看|