欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

The size of WC grains is of great significance to the friction and wear properties of cemented carbide. It is generally believed that coarse-grained cemented carbide has poorer wear resistance than fine-grained cemented carbide. After the grain refinement of cemented carbide, the size of the hard phase decreases, increasing the surface area of the hard phase grains and the bonding force between the grains, and the binder phase is more evenly distributed around them, which can improve the hardness and wear resistance of the cemented carbide. In this paper, the author conducts friction and wear experiments on cemented carbide to analyze the friction and wear properties under different parameters and the material removal mechanism, providing experimental evidence for the optimization design of high-speed cutting tool materials, reasonable material selection, and the study of high-speed cutting wear mechanisms.

Experiment

Test Materials

Three types of WC-6Co cemented carbide with different grain sizes were selected for the test. The size of the cemented carbide disc was φ55mm×4mm, and the surface was rough ground, finely ground, and polished. The mating material used was Al?O? balls with a diameter of 9.5mm. Both samples were ultrasonically cleaned in acetone for 20 minutes and dried for use. The material properties are shown in Table 1.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 2

Friction and Wear Test

The test was conducted on a UMT-2 multi-functional friction and wear testing machine produced by CETR Corporation in the United States, using a ball-on-disc contact method. The structure of the testing machine is shown in Figure 1. The cemented carbide friction disc was attached to the working table with double-sided tape, and the Al?O? ball was placed in the fixture. The two types of mating materials produced mutual movement and force of action. The friction force generated was detected by the sensor, and the curves of friction force, normal force, and friction coefficient were automatically generated by the related software according to Coulomb’s law.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 3

The test was conducted at room temperature, with normal forces of 10N and 20N respectively, and the linear velocities of the friction pair sliding were 40m/min, 80m/min, 120m/min, and 160m/min. The sliding distance was 500m. After the test, a scanning electron microscope (SEM) was used to observe the wear scar surface morphology of the upper and lower samples, and an X-ray energy dispersive spectrometer (EDS) was used to detect the elemental composition of the worn surfaces. All samples were analyzed for the elemental composition of the friction and wear surfaces under the same conditions.

Results and Analysis

Friction and Wear Performance

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 4

Figure 2 shows the friction coefficient curve of ZH cemented carbide drawn by the testing machine’s accompanying software (load 20N, sliding speed 160m/min). The experiment found that each friction process follows a similar pattern, that is, the initial dynamic friction coefficient undergoes a rapid increase from the initial value during the transition period, and then remains relatively stable, showing a fluctuating characteristic in the stable phase. In the beginning, under the action of the normal load, only local micro-convex bodies on the friction surface are in contact, the adhesive area is small, and the molecular attraction on the contact surface is weak, so the friction coefficient is small; as the friction process progresses, the micro-convex bodies interfere with each other, gradually get worn down, the adhesive area increases, and the molecular attraction also increases, leading to a gradual increase in the friction coefficient. The entire friction process is a continuous process of the contact surface adhering and then being sheared under the action of shear stress. Due to the peeling and breaking of the Co phase on the surface, the wear of the sample surface occurs, and the local adhesion on the surface quickly reaches a dynamic equilibrium, resulting in the friction coefficient of the surface being maintained within a relatively stable range, which is called the stable period.

Most scholars use the average value of the friction coefficient over a period of time (distance) as a characterization parameter of friction behavior. Therefore, this experiment selects the average value during the stable friction phase as the friction coefficient of the cemented carbide under the corresponding parameters. Figure 3 shows the friction coefficients of three types of cemented carbide under different loads and speeds.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 5

It can be seen that with the increase of friction speed and load, the friction coefficient of the cemented carbide generally shows a decreasing trend, and the decrease is most obvious in the transition from relatively low speed (40m/min and 80m/min) to high speed (120m/min and 160m/min). From the perspective of material, the friction coefficient of ZH cemented carbide is smaller than that of the other two materials, and the friction coefficients of ZHX and HG cemented carbides are not significantly different, with the friction coefficient of HG cemented carbide being slightly larger.

Wear Mechanism

After the friction and wear tests, the microstructure of the worn surfaces of each sample was observed using a scanning electron microscope (SEM), and SEM images were taken, along with an analysis of the surface composition. The friction and wear mechanisms of the cemented carbide under different friction parameters are similar, as shown in Figure 4 (sliding speed 160m/min, load 20N).

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 6

In the initial stage of cemented carbide wear, the binder phase Co undergoes plastic deformation, and the surface layer of Co is extruded by the WC grains. Due to the low hardness and good ductility of Co, under certain conditions, a micron-scale friction film can form on the surface, while the harder WC particles gradually protrude from the friction surface, preventing further rapid wear of the surface and allowing the friction process to enter a relatively stable stage. As the binder phase Co continues to be lost, the WC framework of the material is damaged, and the dislocation density within the WC particles significantly increases. When the dislocation density accumulates to a certain extent, microcracks will form on the WC particles, causing the WC particles to begin to pull out from the cemented carbide matrix. The detached WC particles remain in the wear area, transforming into abrasive particles, which, under the action of the load, compress against the matrix, resulting in new plastic deformation and grain damage.

cemented carbide

As can be seen from Figure 4, as the grain size of the cemented carbide decreases, the grain density increases, and the degree of surface wear decreases. The surface of the ZHX cemented carbide shows no obvious shedding of WC particles, while the surface density of HG is very good, with almost no obvious shedding of WC particles. Therefore, for the traditional grain size cemented carbide ZH, the main wear mechanism is abrasive wear caused by the extrusion of the binder phase Co and the shedding of WC grains. As the grain size decreases and the density of the fine-grained cemented carbide increases, the phenomenon of WC grain spalling decreases, Co still wraps around the WC, the microstructure of the material remains intact, and most grains only undergo a certain degree of plastic deformation.

Вывод

The size of WC grains has an important effect on the friction and wear properties of cemented carbide. As the grain size decreases, the friction coefficient slightly increases, and the wear resistance is enhanced.

The friction coefficient of cemented carbide is influenced by speed and load, and it shows a decreasing trend with the increase of speed and load.

The wear mechanism of traditional grain size cemented carbide is mainly characterized by the extrusion of the binder phase Co and the fracture and spalling of the hard phase WC grains; the grain spalling phenomenon of fine-grained cemented carbide is not obvious, and the main wear mechanism is plastic deformation.

Добавить комментарий

Ваш адрес email не будет опубликован. Обязательные поля помечены *

91免费精品国自产拍偷拍-亚洲中文字幕av一区二区三区-av男人的天堂在线免费观看-青草视频在线播放免费| 久久亚洲道色综合久久-国产伦精品一区二区三区精品-97人妻精品一区二区三区香蕉-久久精见国产亚洲av高清热| 亚洲中文高清在线观看-久久久国产精品亚洲专区91-中文字幕免费一区二区三区乱码-国产成人精品国内自产拍在线| 久久精品国产亚洲av试看-风韵饥渴的中年富婆偷人视频-99久久久精品国产美女-日本高清av一区二区三区| 国产露脸精品国产人妻-国产精品三级一区二区久久久-久久青草亚洲AV无码麻豆-国产蜜臀av在线一区二区三区| 色成年激情久久综合国产-国产精品亚洲av在线观看-熟妇人妻av中文字幕老熟妇-日韩乱码一区二区三区中文字幕| 狠狠躁夜夜躁人人爽野战天天-91密桃精品国产91久久-欧美亚洲另类久久综合-亚洲精品中文字幕视频在线| 丰满少妇被粗大猛烈进人高清视频-中文字幕亚洲精品乱码在线看-91麻豆精品成人免费视频-好爽好硬好深好大好紧视频| 熟女人妻一区二区在线观看-国产欧美激情视频在线观看-最新亚洲av网址在线观看-毛片在线观看免费日韩| 日本人妻中出一区二区三区-av一区二区三区中文字幕-午夜精品妇人在线观看视频-久热在线观看精品视频| 人妻少妇精品性色av免费-国产精品自拍av一区二区-亚洲欧美国产另类91综合-在线观看国产高清自拍| 中文字幕一区二区成人熟女-在线观看日韩国产亚洲-精品久久人人做人人爽综合-国产精品av一区二区三区| 伊人精彩视频在线免费观看-欧洲精品码一区二区三区免费看-97黄色成人在线网站-国产av无遮挡屁股喷水| 天天日天天射天天好逼-精品露脸贵在真实在线播放-人妻熟妇乱又伦精品视频少妇-国产精品av在线观看免费| 免费亚洲成人av在线播放-日本av一区二区三区四区-久久久精品人妻一区二区三区色秀-雪白大屁股在线观看视频| 部长与人妻日本中字在线-国产午夜福利在现观看-日本老女优五十路中文字幕-69视频在线观看快操我| 黄色av免费在线观看亚洲-国产成人精品一区二区三区免费-国产av大全一区二区三区-国产精品一区二区av白丝在线| 天天日天天射天天好逼-精品露脸贵在真实在线播放-人妻熟妇乱又伦精品视频少妇-国产精品av在线观看免费| 亚洲无人区乱码中文字幕首页-亚洲欧美国产日韩丝袜美腿-国产久久精品一区二区亚洲-疯狂进入丝袜人妻一区二区| 日韩人妻久久精品一区二区-美女露脸多p视频在线观看-中国美女无套免费内射视频-国产最新自拍视频在线观看| av在线免费观看免费-亚洲成av人片一区二区三区-国产裸体露出视频在线观看-亚洲精品成人久久久影院| 亚洲制服丝袜欧美另类-日韩女优在线一区二区三区-国产伦久视频免费观看视频-少妇挑战三个黑人还被内射| 国产一级—片内射视频播放-丰满少妇被粗大猛烈进人高清-精品深夜视频在线观看-亚洲一区二区中文字幕啪啪| 久久久婷婷成人就要色成人-亚洲中出视频在线观看-亚洲精品中文字幕有码-免费男女做爰免费视频| 高潮喷水亚洲精品视频-中文字幕乱码在线高清完整版-韩国三级永久免费看片-狠狠躁夜夜躁人爽碰人妻视频| 在线观看视频免费完整版在线播放-人妻夜夜爽精品波多野-伊人之国产在线观看av-娇妻少妇被躁爽到高潮av| 91精品国产成人一区二区-白丝老师好紧好爽好湿作文-国产成人久久流白浆图-丰满少妇猛烈进出高清晰视频| 在线观看三级午夜福利视频-中文字幕av乱码一区二区三区-国产精品视频自拍视频-伊人久久大香线蕉成人综合网| 熟妇人妻无乱码中文字幕麻-中文字幕在线中文乱码怎么解决-av成人久久精品一区二区-国产精品人妻熟女av久久网址| 久久久婷婷成人就要色成人-亚洲中出视频在线观看-亚洲精品中文字幕有码-免费男女做爰免费视频| 女厕偷窥一区二区三区在线-五月婷婷伊人中文字幕-一个人免费完整视频高清-中文字幕人妻在线一区二区三区| 在线观看视频免费完整版在线播放-人妻夜夜爽精品波多野-伊人之国产在线观看av-娇妻少妇被躁爽到高潮av| 又紧又爽又深精品一区二区-五月婷婷六月丁香动漫-99国内精品一区二区三区-国产一级男女牲交高潮片| 人妻一区二区三区四区免费-在线亚洲国产网红av-国产成人精品免费视频小-中老年熟妇激情啪啪大屁股| 玩弄漂亮少妇高潮正在播放-亚洲宅女午夜福利视频-丰满少妇粗大猛烈进高清播放-黄色亚洲精品大全在线观看| 丰满少妇被粗大猛烈进人高清视频-中文字幕亚洲精品乱码在线看-91麻豆精品成人免费视频-好爽好硬好深好大好紧视频| 黄色av免费在线观看亚洲-国产成人精品一区二区三区免费-国产av大全一区二区三区-国产精品一区二区av白丝在线| 天堂最新在线资源欧美-97超碰人人模人人爽人人爱-免费久久99精品国产婷婷六月-看香蕉视频一直看一直爽| 三级成人艺术视频在线播放-欧美激情午夜视频在线-国产精品亚洲美女久久一区-僧侣之夜无打码无删减高清| 熟妇人妻无乱码中文字幕麻-中文字幕在线中文乱码怎么解决-av成人久久精品一区二区-国产精品人妻熟女av久久网址| 我的美女姐姐完整版在线观看-国产精品一级亚洲av第二区-国产精品亚洲av一区三页-国产成人精品三级在线中文|