High-energy ball milling is the simplest and most effective to produce ultrafine cemented carbide materials, mainly due to two aspects: one is the production of ultrafine or even nanoscale powders, and the other is the inhibition of grain growth during sintering. To prepare high-quality cemented carbide, not only must the particle size of the powder raw material be controlled at the micro-nano level, but the particle size distribution must also be narrow. Moreover, control of the phase structure of the alloy, especially carbon control, is also crucial.. Therefore, this paper will study the use of high-energy ball milling to prepare raw material powders for cemented carbide, and then obtain ultrafine cemented карбид through pressing and sintering methods. This paper will investigate the role of high-energy ball milling and the influence of ball milling conditions on powder particle size.

Main Preparation Techniques for Micro-Nano Cemented Carbide Powders:

1.Low-Temperature Reduction Decomposition Method

This method is an improved version of the conventional reduction carburization method to prepare micro-nano cemented carbide powders. It uses a low-temperature hydrogen process to reduce tungsten acid, tungsten oxide, or tungstic acid to micro-nano-scale tungsten powder, followed by carburization of the tungsten powder to micro-nano-scale WC powder at low temperatures.

2.Mechanical Alloying (MA)

This is a traditional method using mechanical force for the chemical synthesis of micro-nano cemented carbide powders. It involves placing a certain proportion of elemental powder mixtures in a ball mill jar and subjecting them to high-energy ball milling under an inert atmosphere for a long time. The powder particles undergo repeated grinding, breaking, extrusion, cold welding, and low-temperature solid-state chemical processes under the action of mechanical force, resulting in alloy powders with uniform composition and structure.

3.Spray Drying Method

Also known as thermochemical synthesis, this is currently the main method for industrial mass production of WC-Co composite powders. The process was developed by L.E. McCandlish and B.E. Kear of Rutgers University and has been patented. The Nanodyne Company in the United States uses this process to produce nanoscale WC-Co powder with a particle size of 20~40nm. The process involves mixing ammonium metatungstate [(NH?)?(H?WO??O?o)·4H?O] aqueous solution with cobalt chloride (CoCl·nH?O) to form an original solution, which is then atomized and dried to form a uniformly composed, fine mixture of tungsten and cobalt salts, followed by reduction and carburization in a fluidized bed to obtain nanophase WC-Co powder.

4.Gas Phase Reaction Method

This method uses the principle of gas-phase chemical reaction deposition to produce powders. It involves evaporating and vaporizing metals or alloys in equipment and reacting with active gases at certain temperatures to produce metal compounds, which are then condensed to obtain micro-nano-scale compound powders.

 

Experimental Method

High-purity cobalt powder and 0.8μm tungsten carbide powder were used as raw materials, mixed in a WC-10%Co ratio, and subjected to high-energy ball milling with a ball-to-material ratio of 9:1 using a QM-IF type planetary ball mill. The ball milling time was set at 24 hours per interval, with milling times of 24, 48, 72, and 96 hours. The particle size of the milled powder was measured using the Fsss method and X-ray diffraction. The powder samples with different ball milling times were then pressed and sintered under the same conditions to prepare cemented карбид specimens. Subsequently, strength and hardness tests were conducted, along with metallographic analysis.

 

Results and Analysis

The Influence of Ball Milling Time on Powder Particle Size and Grain Size

Table 1 shows the measured Fsss particle sizes. It can be seen that the powder particle size decreases with the extension of ball milling time but becomes coarser after decreasing to a certain extent. However, the grain size continuously decreases. Powder particles and grains are different concepts. Particles consist of multiple grains encapsulated by cobalt powder. As ball milling progresses, while powder particles break, cold welding can also occur between the cobalt on the particle surfaces. Therefore, when ball milling reaches a certain degree, particle agglomeration exceeds breaking, leading to an increase in particle size, which eventually maintains a certain equilibrium state. The measured grain size is usually WC grains, which are brittle phases and easily broken during ball milling. Due to the encapsulation by cobalt powder, it is difficult for WC grains to cold weld, so the grain size continuously decreases.

Study on the Preparation of Ultrafine Cemented Carbide by High-Energy Ball Milling 2

Study on the Preparation of Ultrafine Cemented Carbide by High-Energy Ball Milling 3

Microstructure After Sintering

Figure 3 shows the metallographic structure obtained after sintering, clearly indicating the influence of ball milling time on the grain size, shape, and distribution. As the ball milling time extends, the grains in the sintered body are significantly refined, tend to be uniform in size, and the WC grains are more dispersed. This is due to two factors: first, the WC grains themselves are refined and homogenized through ball milling, indicating that ball milling not only breaks the WC grains but also homogenizes them; second, it is formed during the sintering process. The sintering process only coarsens the particles and causes non-uniformity due to abnormal grain growth, which typically becomes more severe with longer ball milling time, as ball milling can cause lattice distortion, promoting abnormal grain growth. However, the results of this experiment do not show this; instead, the grain size tends to be more uniform with the extension of ball milling time. Clearly, the homogenization of WC grains is due to the effect of ball milling. This demonstrates that high-energy ball milling can refine and homogenize WC grains.

Study on the Preparation of Ultrafine Cemented Carbide by High-Energy Ball Milling 4

The Effect of Ball Milling Time on the Mechanical Properties of Ultrafine Cemented Carbide

Tables 1 and 2 show the measured bending strength and hardness, respectively. It can be seen from the tables that both strength and hardness increase with the extension of ball milling time. As previously analyzed, the longer the ball milling time, the finer the WC grains in the sintered samples and the more uniform their distribution. This indicates that bending strength and hardness increase simultaneously with the refinement of grains. In the grain size range above the micron level, the strength and hardness of cemented carbide typically have an inverse relationship; that is, as bending strength increases, hardness decreases, and vice versa. However, in this case, both have improved simultaneously, which clearly shows that after high-energy ball milling, the obtained cemented carbide has reached the micro-nano scale grain size range. The hardness improvement of the cemented carbide in this study is very significant; generally, WC-10%Co has a hardness of about HRA91, but here it has reached as high as 92.8. This indicates that grain refinement has a very strong strengthening effect on cemented carbide.

Study on the Preparation of Ultrafine Cemented Carbide by High-Energy Ball Milling 5

Вывод

This paper has conducted a preliminary study on the relationship between ball milling time and grain size in WC-Co ultrafine cemented carbide, as well as the relationship between grain size and strength, hardness, and the following conclusions are drawn:

High-energy ball milling has a very strong breaking effect on WC grains, and the WC grain size refines with the increase of ball milling time. However, there is a critical point for the powder particle size during ball milling. Upon reaching this critical point, the grain size of the cemented carbide is the smallest, after which, with the increase of ball milling time, the grains may become coarser instead.

Micro-nano grain size cemented carbide can be obtained through high-energy ball milling, and the WC grains are more uniform and dispersed.

The refinement of the grain size of cemented carbide to the micro-nano scale can simultaneously increase the bending strength and hardness.

Добавить комментарий

Ваш адрес email не будет опубликован. Обязательные поля помечены *

国产日韩电影一区二区三区-美女露双奶头无遮挡物| 国产欧美成人精品第一区-日本黄色精品一区二区| 久艹在线观看视频免费-人妻偷人精品一区二区三区| 国产aa视频一区二区三区-国产精品久久久久久久毛片动漫| 蜜臀av日日欢夜夜爽一区-av在线免费永久播放| 欧美日韩国产亚洲免费-肉体粗喘娇吟国产91| 青青操大香蕉在线播放-国产亚洲欧美精品在线观看| 国产精品久久99精品毛片-国产四季高清一区二区三区| 国产剧情av中文字幕-五月婷婷在线手机视频| 性激烈欧美三级在线播放-久久中文字幕人妻少妇| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 一区二区三区女同性恋-熟妇高潮一区二区高清网络视频| 一区二区国产高清在线-日本高清无卡一区二区三区| 性色国产成人久久久精品二区三区-偷窥中国美女洗澡视频| 国产av一区二区三区日韩接吻-av网址在线播放网站| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| av噜噜国产在线观看-欧美视频亚洲视频一区二区三区| av一区免费在线观看-中文字幕日韩国产精品视频| 国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 久久精品亚洲国产av久-国产精品视频一区二区免费| 亚洲国产中文欧美一区二区三区-国产精品一区二区视频成人| 国产在线一区二区三区欧美-久久偷拍精品视频久久| 日韩亚洲欧美综合在线-成人在线网站在线观看| 午夜福利卫生纸福利院-一区二区三区久久亚洲| 夜夜久久国产精品亚州av-欧美大屁股一区二区三区| 国产精品熟女视频一区二区-国产日韩精品欧美一区喷水| 性都花花世界亚洲综合-日韩av一区二区三区| 久久精品人妻一区二区三区极品-久久99热这里只有精品免费| 亚洲一区二区免费av-中文字幕人妻久久久一区二区三区| 日韩二级视频在线观看-美女扒开奶罩露出奶子的视频网站| 亚洲综合av一区二区三区-高潮又爽又黄无遮挡激情视频| 欧美精品国产系列一二三国产真人-在线观看国产午夜视频| 91九色蝌蚪丝袜人妻-国产精品9999网站| 黄片免费观看视频下载-国产丝袜诱惑在线视频| 性激烈欧美三级在线播放-久久中文字幕人妻少妇| 久久人妻一区二区三区欧美-国内不卡的一区二区三区| 深夜三级福利在线播放-日韩精品一区二区在线天天狠天| 国产精品一区二区欧美视频-国产一区二区三区天码| 人妻少妇无乱码中文字幕-人成免费视频一区二区| 人妻少妇无乱码中文字幕-人成免费视频一区二区| 91亚洲美女视频在线-熟妇人妻精品一区二区三区蜜臀|