A sinteriza??o de metal duro é uma etapa crucial na produ??o de metal duro. Durante o processo de prensagem do pó de metal duro, a liga??o entre as partículas do pó depende principalmente da press?o exercida durante a prensagem, e as partículas do pó n?o podem se ligar umas às outras devido à falta de tens?o de escoamento. O compacto prensado existe num estado poroso. O método de sinteriza??o em fase líquida da metalurgia do pó é necessário para a sinteriza??o. Existem principalmente vários métodos de sinteriza??o para carboneto: sinteriza??o de hidrogênio, sinteriza??o a vácuo, sinteriza??o de baixa press?o e prensagem isostática a quente. O equipamento também varia de acordo com os diferentes processos e métodos de sinteriza??o.

The State of Carbide Compact Formation

After the carbide?compact is formed, it exists in a porous state. During the wet grinding process, the shape of WC is subjected to strong impacts, resulting in increased surface energy and enhanced reactivity. The longer the contact time of the compact with air, the greater the degree of oxidation, requiring more carbon for reduction. With the theoretical carbon content of carbide?remaining at 6.128%, the ratio of oxygen atoms to carbon atoms is 12/16. Therefore, for every additional unit of oxygen, it will consume 3/4 of the carbon content. This leads to the formation of the η phase more easily after alloy sintering.

The Existence of Oxygen in Carbide Mixtures

The oxygen content in the carbide?mixture can be considered to exist in three forms: occluded oxygen, cobalt surface oxygen, and oxygen in WO2 or WO3. Since the oxygen content measured by chemical oxygen determination includes the total of these three types of oxygen, it is difficult to determine their respective proportions in production. Therefore, this poses challenges to production. Additionally, oxygen enrichment in the environment is ubiquitous, so it is essential to manage each process reasonably in actual production.

Occluded Oxygen

Exists in the interstices of the compact and on the surface of the compact and mixture; generally removed by vacuum evacuation at the beginning of sintering, so it does not affect alloy sintering.

Cobalt Surface Oxygen

Due to the high susceptibility of cobalt to oxidation at room temperature, oxidation intensifies with increasing temperature. After wet grinding and subsequent drying, a layer of oxide film forms on the cobalt surface; the longer the material or compact is stored before sintering, the higher the degree of cobalt oxidation. This portion of the oxide requires carbon for reduction; before the temperature reaches 600°C during sintering, reduction mainly relies on free carbon, and the remaining unreduced oxides must be reduced by combined carbon. This portion of oxygen is critical to the carbon-oxygen balance during alloy sintering and is difficult to control.

WO2 or WO3 Oxygen

Also known as compound oxygen; before the carbonization of WC, WO3 gradually transforms into WO2 and then into tungsten powder (W), followed by carbonization. Some oxides may remain incompletely reduced or partially oxidized due to storage time, from W → W2C → WC, and may persist even after completion. Alternatively, inadequate protection during storage may lead to oxidation. These oxide residues are referred to as compound oxygen; the reduction temperature generally occurs before 1000°C, but severe oxidation may delay reduction until 1200°C. This oxide residue consumes carbon significantly, narrowing the margin for carbon levels and making it difficult to control sintering carbon content, thereby complicating the achievement of sufficient liquid phase formation.

 

The Form of Carbon in carbide

The carbon content in carbide?mainly exists in three ways: WC stoichiometry, carbon increment from binder decomposition, and carbon infiltration from furnace gases.

Generally, WC is adjusted according to the theoretical carbon content of carbide; reasonable carbon adjustment is made based on small samples before wet grinding; in the wax process, the carbon content is adjusted by subtracting the amount of carbon infiltrated from furnace gases and adding the amount of carbon consumed by oxides. In the rubber process, one-third of the rubber weight should be subtracted.

Carbon Increment from Binder Decomposition

During debinding and sintering, whether using wax, PEG, or rubber, there is more or less decomposition; thus, carbide?can gain carbon, although the amount of carbon increase varies with different binders. Since wax mainly relies on evaporation, it is generally considered not to increase carbon content. On the other hand, rubber and PEG rely on decomposition, with rubber decomposition occurring at higher temperatures, resulting in more carbon increase.

carbide metal

Carbon Infiltration from Furnace Gases

Since most heating elements, insulation layers, sintering plates or boats in carbide?sintering furnaces are made of graphite products, their effects become evident at 600°C; when sintering temperature rises above 1200°C, a large amount of carbon and CO released from graphite exacerbate carbon infiltration into carbide.

Impact of Cobalt on carbide?Properties

Cobalt has a hexagonal close-packed crystal structure, making it highly reactive and prone to oxidation. In WC-Co alloys, cobalt acts as the binder metal. When the cobalt phase exhibits the ε-Co crystal structure, with fewer slip planes (theoretically no more than 3), the alloy’s toughness is low. However, when the cobalt phase exhibits the α-Co crystal structure, the maximum number of theoretical slip planes can increase to 12, resulting in stronger fracture resistance. With increasing sintering temperature, the cobalt crystal structure shifts from hexagonal close-packed to face-centered cubic; the reverse occurs during cooling. Since tungsten dissolves more in cobalt, playing a “nailing” role, the transformation of crystal structure during cooling varies with the amount of tungsten dissolved.

Up to 1% of cobalt can dissolve in WC at room temperature; when the sintering temperature reaches between 400°C and 800°C, vigorous diffusion and rearrangement of cobalt occur. During this period, a lower amount of free carbon is more conducive to increased slip planes; this is advantageous in wax processes. However, rubber processes require completion of decomposition around 600°C, affecting the effective occurrence of cobalt phase slip planes.

At 1000°C during sintering, the oxide has almost completed the reduction process, so this stage is referred to as oxygen-free sintering. Carbon content in carbide?is generally tested at this stage; however, the so-called oxygen-free carbon contains only a minimal amount of oxygen. Nonetheless, oxide on the cobalt surface has been completely reduced by this point, and the edges of the cobalt phase have produced fewer liquid phases. At this stage, the compact has acquired some hardness, known as the pre-sintering stage. Products at this stage can undergo plastic processing if necessary.

The Sintering Mechanism of?Carbide 2

Liquid Phase in Carbide

Theoretically, the liquid phase in WC-Co alloys appears at 1340°C. The temperature at which the liquid phase sufficiently appears varies with carbon content. As sintering temperature rises, the amount of liquid phase increases; fine WC particles gradually form a liquid phase. Intense shrinkage occurs in the product, reducing the distance between WC particles. Fine WC particles are gradually melted by larger particles, resulting in coarser WC particles. This phenomenon is known as grain growth. Grain growth during sintering is inevitable, particularly in ultrafine or submicron WC, where grain growth is more pronounced. To effectively inhibit excessive grain growth, inhibitors such as VC, TaC, and Cr3C2 can be added.

After sintering, undissolved WC and W2C rapidly precipitate, followed by ternary eutectic formation, laying the foundation for the alloy. The longer the cooling time above 1200°C, the more complete the precipitation, but the greater the opportunity for grain growth.

O mecanismo de sinteriza??o do carboneto 3

Conclus?o

The pursuit of ternary eutectic structures is the most critical aspect of sintering in WC-Co carbide. Ternary eutectic structures form the fundamental framework of carbide. In the W-C-Co ternary system, effective handling of WC grain growth, allowing more tungsten to dissolve in cobalt without decarburization, thereby improving the durability and toughness of carbide, is always the goal of alloy manufacturers. A German technical expert once said: “The essence of sintering lies in ‘high temperature and low carbon’.”

Deixe uma resposta

O seu endere?o de e-mail n?o será publicado. Campos obrigatórios s?o marcados com *

国产欧美一区二区三区嗯嗯-欧美一区二区日本国产激情| 哦啊好大用力欧美视频-麻豆国产传媒片在线观看| 欧美亚洲另类久久久精品-国产精品一区二区亚洲推荐| 欧美三级韩国三级日本三斤-日本不卡一区不卡二区| 亚洲产国偷v产偷v自拍性色av-亚洲欧美日韩国产三区| 国产精品一区二区在线免费-久久精品国产亚洲av热明星| 男女做爰猛烈啪啪吃奶在线观看-人妻连裤丝袜中文字幕| 国产av剧情护士麻豆-三级国产精品欧美在线观看| 亚洲永久免费在线观看-亚洲欧美导航一区二区导航| 国产日韩电影一区二区三区-美女露双奶头无遮挡物| 国产综合日韩激情在线-日韩精品人妻一专区二区三区| 欧美字幕一区二区三区-好吊妞欧美一区二区在线观看| 少妇一区二区三区粉嫩av-国产精品区久久久久久久| 免费看黄色污污的网站-欧美一区二区三区爽爽| 国产精品美女在线网址-久草免费福利在线观看视频| 国产日韩电影一区二区三区-美女露双奶头无遮挡物| 青青操大香蕉在线播放-国产亚洲欧美精品在线观看| 丝袜高跟熟女视频国产-熟女少妇亚洲一区二区| 欧美精品午夜一二三区-a屁视频一区二区三区四区| 久艹在线观看视频免费-人妻偷人精品一区二区三区| 国产免费高清av在线播放-成年人在线播放中文字幕| 亚洲区欧美区在线视频-亚洲碰碰人人AV熟女天堂| 成人免费资源在线观看-欧美国产日韩高清在线综合| 在线国产自偷自拍视频-蜜桃a∨噜噜一区二区三区| 国模自慰一区二区三区-日韩一级黄色片天天看| 一区二区国产高清在线-日本高清无卡一区二区三区| 亚洲最新国产无人区123-黄片一区二区在线观看| 日韩国产一区二区三区在线-精品日韩人妻少妇av| 欧美一级二级三级在线看-日韩精品欧美嫩草久久99| 国产精品中出久久久蜜臀-久久久中国精品视频久久久| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 亚洲国产中文欧美一区二区三区-国产精品一区二区视频成人| 亚洲午夜久久久精品影院-性感美女在线观看网站国产| hd在线观看一区二区-免费一区二区三区毛片在线| 中文字幕亚洲中文字幕-丰满老妇伦子交尾在线播放| 人妻少妇无乱码中文字幕-人成免费视频一区二区| 天天日天天干天天综合-99久久综合狠狠综合久久| 天天干天天干2018-91人妻人人澡人爽精品| 乱入一二三免费在线观看-久久精品亚洲精品国产色婷婷| 国产成人精品免费视频大全办公室-亚洲欧美日本综合在线| 极品人妻av在线播放-久久精品视频一区二区三区|