CNC drilling machines and carbide micro drills have always been the mainstream equipment for processing PCB circuit boards. A large amount of PCB processing tasks still rely on CNC milling and drilling to complete. As a subsystem of electronic products, PCB circuit boards play a role as a core module unit. Modern high-performance electronic products have increasingly higher requirements for PCBs, which also means that the precision requirements for carbide micro drill are becoming higher and higher.

 

Common PCB substrate copper laminates are made by bonding the insulation material and copper foil using adhesive and hot pressing, with epoxy glass fiber cloth board used as a pressure plate reinforcement material.? The board contains uncured resin, and the heat generated by mechanical friction during processing will soften the uncured resin, increasing frictional resistance, breaking cutting tools, and producing sludge, which affects processing quality. This makes the mechanical processing performance of PCB boards relatively poor.

This article mainly compares and studies the cutting performance of carbide ?drills produced by our company in China and similar famous carbide ?drills abroad when processing PCB boards.

 

Test Conditions

The test selected drills of the same specifications but from different manufacturers to drill holes in PCB boards. The selected tool specifications are shown in Table 1.

carbide micro drill bit

To reduce the impact of experimental errors, four tools from two companies were selected for drilling experiments. The material being cut was a double-layer copper PCB with a thickness of 1.2mm, and a 2.5mm thick cardboard was placed underneath the work piece.

During the processing, the cutting performance of the tools from the two companies was compared by comparing the roughness and chip removal of the processed PCB board, as well as the tool life.

 

 

Experimental Data

Test PCB Machining Quality

The machining quality of the PCB boards observed after cutting with 8 different drill bits is shown in Table 2. It can be seen that the 4 drill bits from Meetyou company can generally achieve good machining results, except for the fourth bit which caused sawtooth-like defects on the PCB board. In comparison, two of the foreign company’s drill bits caused corrugated defects and sawtooth-like defects on the PCB board. The surface roughness of the PCB board after machining can also indicate that the micro drill from Meetyou company have better surface roughness during the machining process, while the drill bits from the foreign company have poorer surface roughness on the PCB board after machining. However, compared with the drill bits from Meetyou company, the chip removal effect of the drill bits from the foreign company is not as good.

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 2

PCB Carbide micro drill’s service life

The average service life of 8 drill bits from Company 2 can be seen from Figure 3. It can be seen that the service life of Meetyou Company’s drill bits is about 40% higher than that of the drill bits from a foreign company.

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 3

 

From Table 4, it can be seen that the lifespan values of the eight drills from the two companies are in a discrete distribution, with almost 40% difference in the lifespan of the same company’s drills. This shows that even though Meetyou’s drills have better quality, from the experiment we can see that there is still much room for improvement in the tungsten carbide micro drills of both companies.

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 4

 

The experimental results showed that the surface roughness and tool life of the PCB board processed by Meetyou’s drill bit were better than those of the foreign company, but the tool life of both companies was not consistent. The photographs of the tools after processing showed that the main forms of tool wear were caused by the generation of abrasive particles and surface oxidation wear.

 

Problems Generated by carbide micro drill on?PCB Circuit Boards

Through high-speed photography to observe the drilling process and the chip removal situation, scanning electron microscopy to observe the drilling morphology, and using software such as Deform and AdvantEdge FEM to simulate the drilling process extensively, it was found that the drilling process of PCB circuit boards is not simply punching holes, but a conventional metal cutting process. It will form conical spiral chips, and the copper chips will bend and break under the action of gravity during the discharge process, and finally be thrown out at high speed rotation of the micro drill, as shown in Pic. 1.

The epoxy resin glass fiber cloth chips are discharged in the form of white powder. The resin in the chips is easy to soften under heating conditions, and the glass fiber chips are adhered together to form mixed chips, as shown in Pic. 2. This kind of mixed chips are easy to adhere to the hole wall and form drilling dirt, which will also adhere to the drill tip and affect the next drilling step, and may even adhere to the spiral groove surface to obstruct chip removal. The drilling models of micro drilling for copper foil and epoxy glass fiber cloth are shown in Pic.3.

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 5

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 6

 

Reasons analysis to cause drilling problems on PCB

Drilling force

The drilling force fluctuated significantly during the drilling of epoxy glass fiber cloth with micro-drills, which was due to the small size of the micro-drills. When drilling glass fibers, the axial drilling force decreased sharply with the fracture of the glass fibers because the micro-drill only drilled a few glass fibers at the same time. The axial force and torque both decreased with increasing speed, but increased with increasing feed rate and core thickness. With an increase in helix angle, the axial force increased, while the torque decreased. The typical drilling process of a micro-drill with a diameter of 0.1mm is shown in Figure 4.

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 7

Drilling temperature

The temperature at the moment of drilling a PCB with micro-drills was measured using an infrared thermal imager and extensively simulated. The results showed that the drilling temperature was typically below 80°C at the moment of drilling with micro-drills. The drilling temperature decreased with an increase in feed rate and spindle speed, but increased with an increase in the number of drill holes and the diameter of the micro-drill. The drilling temperature measured by the infrared thermal imager is shown in Figure 5.

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 8

Drill bit wear

the morphology of micro-drill wear was observed through scanning electron microscopy, as shown in Figure 6. The wear characteristics of micro-drills are mainly abrasive wear and adhesive wear. Abrasive wear mainly occurs on the transverse edge and main cutting edge, affecting the service life of micro-drills. Glass fibers and fillers in PCBs are the main cause of abrasive wear in micro-drills. Resin-mixed chip adhesion wear occurs on the drill tip and helix groove surface of micro-drills, as shown in Figure 7, which affects the cutting performance and chip removal of micro-drills, thereby causing the temperature inside the hole to accumulate and aggravating micro-drill wear.

5 Common Machining Quality Issues of carbide?micro drill on?PCB? 9

  1. D=0.1 mm,vf=150cm/min,n=295/min,vr=2300cm/min,2500holes.
  2. D=0.2mm,vf=150cm/min,n=155/min,vr=1800cm/min,1500holes.
  3. D=0.3mm,vf=240cm/min,n=145/min,vr=1800cm/min,1500 holes

Fracture

It?was found that the fracture was caused by the edge near the drill tip participating in cutting during processing, which is easily damaged by friction and impact of glass fiber, causing cutting to not proceed normally. Micro-drill bending and severe twisting ultimately lead to micro-drill breakage. Experimental and simulation results show that excessive twisting load is the main cause of micro-drill breakage, and the fracture point of the micro-drill is located at the root of the micro-drill spiral groove, at a certain distance from the top of the drill.

Conclusion?of carbide micro-drill’s drilling quality for PCB.

In summary, by observing the micro-hole sections under scanning electron microscopy, it was found that not only are there entrance and exit burr problems on the micro-hole surface, but also entrance roundness error, entrance size error, burrs and hole position accuracy, and roughness of the hole wall. The burrs and edges of micro-drills are mainly caused by micro-drill wear. Roughness of the micro-hole wall mainly occurs due to the fracture and shedding of multiple glass fibers in the epoxy glass fiber layer. Hole position accuracy is mainly related to spindle vibration characteristics, drill diameter, and drill wear. Reducing feed speed and increasing rotation speed can improve the quality of micro-holes in PCBs within a certain number of drilling holes. The most fundamental method to improve micro-hole quality is to reduce the contact area between micro-drills and PCBs to improve the wear resistance of micro-drills.

Deixe uma resposta

O seu endere?o de e-mail n?o será publicado. Campos obrigatórios s?o marcados com *

99在线免费观看视频-丰满人妻一区二区三区视频53| 国产欧美一区二区三区嗯嗯-欧美一区二区日本国产激情| 欧美日韩国产综合四区-爆操极品尤物熟妇14p| 俄罗斯胖老太太黄色特级片-国产精品黑丝美腿美臀| 日韩精品中文在线观看一区-亚洲bt欧美bt精品| 青青草原免费国产在线视频-精品人妻乱码一区二区三区四区| 日韩二级视频在线观看-美女扒开奶罩露出奶子的视频网站| 天天干天天干2018-91人妻人人澡人爽精品| 国内精产熟女自线一二三区-六月丁香婷婷在线观看| 午夜日韩精品在线视频-亚洲网老鸭窝男人的天堂| 99久热精品免费观看四虎-亚洲天堂精品视频在线| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 国产欧美日本一区二区-一区二区三区亚洲在线播放| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 国产精品美女在线网址-久草免费福利在线观看视频| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 亚洲一区二区免费av-中文字幕人妻久久久一区二区三区| 亚洲av高清一区三区三区-久久人妻夜夜做天天爽| mm在线精品视频在线观看-欧美国产日韩在线一区二区三区| 蜜臀av日日欢夜夜爽一区-av在线免费永久播放| 亚洲av日韩五月天久热精品-国产日韩欧美一区二区三区群战| 男人的天堂久久精品激情-最新亚洲精品a国产播放| 哦啊好大用力欧美视频-麻豆国产传媒片在线观看| 国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 天天干天天干2018-91人妻人人澡人爽精品| 色综合色综合久久综合频道-埃及艳后黄版在线观看| 四虎成人在线免费视频-亚洲熟女中文字幕天堂| 一区二区三区国产高清mm-美女张开腿让帅哥桶爽| 亚洲欧美激情自拍色图-国产亚洲精品sese在线播放| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 激情字幕久久久字幕中文-一区二区三区免费黄片| 日本女优一卡二卡在线观看-欧美大胆a级视频秒播| 久久特一级av黄色片-91社区视频免费观看| 欧美日韩国产亚洲免费-肉体粗喘娇吟国产91| 国产欧美日本一区二区-一区二区三区亚洲在线播放| 两性污污视频网站在线观看-亚洲欧美日韩激情一区| 中文字幕日韩精品不卡一区二区-成人av在线观看一区二区| 国产美女网站在线观看-国产精品亚洲综合网69| 国产小黄片高清在线观看-涩涩鲁精品亚洲一区二区| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 91亚洲美女视频在线-熟妇人妻精品一区二区三区蜜臀|