Wet milling can grind hard phases (mainly WC phase) to the required particle size and achieve a uniform mixing state with Co powder in a small range, which has good compaction and sintering properties. Therefore, the wet milling time is also one of the key parameters in the preparation process of hard alloys. This article mainly studies the influence of wet milling time on the microstructure and properties of hard alloys.

Experimental materials for wet milling and methods

The recycled WC-Co composite powder produced by zinc melting method was used as the experimental material, and its composition is shown in Table 1.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci YG8 (ISO K30) W?glik spiekany 2

Laser particle size analysis showed that the median diameter was 3.46μm, with a narrow range of particle size distribution and relatively concentrated particle size. Figure 1 shows the SEM image of the original morphology of the WC-Co composite powder.

Effects of Wet?milling Time on Microstructure and Properties of YG8(ISO K30) Cemented Carbide 3

From Fig.1, it is evident that the recycled powder has mild agglomeration, and its morphology is mostly triangular or rectangular with smooth edges, retaining the characteristics of WC grains in hard alloys. The average particle size of the powder is about 3μm, which is consistent with the results obtained from laser particle size analysis.

 

Figure 2 shows the XRD spectrum of the WC-Co composite powder.

Effects of Wet?milling Time on Microstructure and Properties of YG8(ISO K30) Cemented Carbide 4

Experimental Results and Discussion about wet milling time

Figure 3 shows the morphology of WC-Co composite powders after different wet milling?times. As shown in Figure 3(a), when wet milling?for 18 hours, the powder size is relatively large and unevenly distributed, indicating that the wet milling?effect is not ideal, and the collision between the grinding balls and the powder in the tank is insufficient, and the powder refinement is not enough. After wet milling?for 24 hours (Figure 3(b)), it was found that the powder size decreased rapidly, and the refinement was obvious, but the uniformity was limited. It can be observed that the powder fragmentation mainly occurred due to the repeated impact and friction of the grinding balls, resulting in the rupture of large particles into smaller particles. Continuing wet milling?until 30 hours (Figure 3(c)), it can be found that there is not much change in the powder size, but the uniformity and morphology have improved, with an average particle size between 1 and 2 μm. This indicates that the powder wet ground for 30 hours has a relatively ideal particle size and morphology. Apart from the rupture, the powder is mainly worn out (WC corners are worn out, producing fine powder). Finally, after wet milling?for 36 hours, it is evident that the powder not only did not refine further but also showed agglomeration phenomenon B (see Figure 3(d)).

wet milling time

 

It should be noted that the powder cannot be infinitely refined during ball milling. During ball milling, as the particle size of the powder decreases, the specific surface area of the powder increases exponentially, exhibiting high surface energy and a sharp increase in reactivity, making it easy to agglomerate and bond with other powders to resist the increase in total energy. As a result, on the one hand, external energy is input into the powder, causing it to refine; on the other hand, the powder agglomerates and forms lumps, reducing the system energy. After the combined effect of these two trends, a dynamic equilibrium is reached between them, and the average particle size of the powder will eventually stabilize within a certain range. In this experiment, the powder was ball milled for 30 hours, and its uniformity was good, with a particle size reaching an equilibrium value (1-2 μm).

Figure 4 shows the XRD patterns of sintered regenerated cemented carbide with different wet milling times. As shown in the figure, when wet milled for 18 hours, the alloy contains impurity phase of elemental carbon (C); as wet milling continues, the elemental carbon disappears. This indicates that the alloy is slightly carburized during wet milling for 18 hours, and as the wet milling time is prolonged, the powder is refined and the surface adsorbs more oxygen, resulting in an increase in the oxygen content of the mixture. During sintering, part of the carbon is consumed, resulting in the formation of a pure two-phase structure of WC and Co in the alloy, and no other impurity phases were found.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci w?glika spiekanego YG8 (ISO K30) 5

Figure 5 shows the metallographic images of the cemented carbide after corrosion for different wet milling times. Comparing Figures 5 (a) to (d), it can be seen that under the sintering process (1723 K, pressure), the alloy structure is good, and no defects such as abnormally large WC grains and cobalt pools were found. The grain size of the alloy is slightly smaller with a polygonal morphology after wet milling for 24 hours compared to 18 hours, and the Co phase is evenly distributed. As wet milling continues, there is no significant change in grain size, but the uniformity slightly improves. When wet milled for 36 hours, it was found that the WC grains had slightly grown, which may be related to the partial agglomeration of the powder during wet milling.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci w?glika spiekanego YG8 (ISO K30) 6

It is worth noting that as the wet milling?time increases, the strength of the alloy shows a continuous upward trend, but the magnitude of the increase becomes smaller and smaller. Generally, for the same Co content and without obvious defects, the strength of the alloy is related to the distribution of internal micro-pores and WC grain size. When wet milling?for 18 hours, due to the short time, the material mixing is uneven, the powder refinement degree is insufficient, the particle size is large, and the distribution is uneven, resulting in the easy formation of micro-pores during sintering, thus the alloy strength is not high. Continuing wet milling?further breaks down the powder particles, increases the number of fine WC particles, narrows the WC particle size distribution towards homogenization, and eliminates the coarse WC grains, which are the main sources of cracks, resulting in an increase in the bending strength of the alloy.

In WC-Co alloys with the same Co content, the coercive force of the alloy is inversely proportional to the WC grain size and distribution, which is consistent with the description in Figure 5.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci w?glika spiekanego YG8 (ISO K30) 7

Figure 6 shows the distribution of flexural strength for regenerated cemented carbides with different wet milling times. Based on Figure 6, the range of strength values for each alloy can be observed, which gives the variation of the strength of the statistical samples. It can be seen from the figure that there are many overlaps and dispersions in the experimental results. It is easy to find that with the extension of wet milling time, not only the strength of the alloy increases, but also the fluctuation range becomes narrower, and each strength value is closer to each other. This indicates that the extension of wet milling time can reduce the discreteness of the strength distribution of regenerated cemented carbides.

 

Wniosek

Under the experimental conditions of this study, the effects of different wet milling?times on the microstructure and properties of recycled WC-8Co composite powder and sintered hard alloys were investigated, and the following conclusions were drawn:

  1. Continuous wet millingfor 30 hours with a ball-to-powder ratio of 3:1 resulted in fine and uniformly distributed composite powder with an average particle size of 1-2 μm, as observed by SEM.
  2. Under the conditions of continuous wet millingfor 36 hours with a ball-to-powder ratio of 3:1 and sintering process (1723 K for 1 hour with a pressure of 5 MPa), the alloy exhibited the best comprehensive properties. Its density was 14.71 g/cm3, HRA90.1, the average strength was 3560 MPa, cobalt magnetism was 7.2%, and coercivity was 15.8 kA/m.
  3. The analysis of the strength distribution of alloys with different wet millingtimes showed that within a certain range, the prolongation of wet milling?time can reduce the discreteness of the strength distribution of recycled hard alloys.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

亚洲精品激情一区二区-久久成人国产欧美精品一区二区| 国产精品久久久精品一区-99久久免费精品国产男女性高好| 亚洲精品蜜桃在线观看-国产欧美日韩在线观看精品观看| 精彩亚洲一区二区三区-中文字幕中文字幕在线色站| 一区二区国产高清在线-日本高清无卡一区二区三区| 性色国产成人久久久精品二区三区-偷窥中国美女洗澡视频| 国产老熟女激情小视频-成人一区二区人妻不卡视频| 日本少妇激情一区二区-亚洲自偷自拍熟女另类蜜臀| 亚洲区欧美区在线视频-亚洲碰碰人人AV熟女天堂| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 白嫩美女娇喘呻吟高潮-久久一区二区三区日产精品| 人妻互换精品一区二区-夜夜爽一区二区三区视频| 欧美日本亚一级二级三区久久精品-日韩欧美一区二区久久婷婷| 熟女少妇免费一区二区-麻豆一区二区三区免费在线观看| 亚洲欧美日韩二区三区-国产在线欧美一区日韩二区| 男人的天堂久久精品激情-最新亚洲精品a国产播放| 人妻日韩精品中文字幕图片-麻豆极度性感诱人在线露脸| 国产午夜精品理论片A级漫画-久久精品国产99亚洲精品| 国产日韩电影一区二区三区-美女露双奶头无遮挡物| 亚洲愉拍自拍欧美精品app-亚洲一区不卡在线视频| 黄色av网站在线免费观看-亚洲欧美精品偷拍tv| 97人妻精品一区二区三区爱与-日韩精品亚洲专区在线观看| 中文字幕人妻少妇第一页-隔壁的女孩在线看中文字幕| 日本韩国亚洲欧美三级-日本东京不卡网一区二区三区| 国产精品中出久久久蜜臀-久久久中国精品视频久久久| 国产精品一区二区欧美视频-国产一区二区三区天码| 欧美视频在线观看国产专区-亚洲91精品在线观看| 欧美aa一级视频播放-久一一区二区三区大香蕉| 亚洲精品蜜桃在线观看-国产欧美日韩在线观看精品观看| 国产欧美成人精品第一区-日本黄色精品一区二区| 国产欧美日本不卡精美视频-日本后入视频在线观看| 中文字幕亚洲中文字幕-丰满老妇伦子交尾在线播放| 99在线免费观看视频-丰满人妻一区二区三区视频53| 亚洲产国偷v产偷v自拍性色av-亚洲欧美日韩国产三区| 国产传媒中文字幕在线观看-午夜福利视频在线播放观看| 亚洲精品在线观看一二三区-在线观看国产中文字幕视频| 亚洲av成人一区国产精品网-国产偷_久久一级精品a免费| 亚洲精品激情一区二区-久久成人国产欧美精品一区二区| 一区二区三区女同性恋-熟妇高潮一区二区高清网络视频| 亚洲视频一区二区三区免费-国产一级黄色大片在线| 亚洲欧洲一区二区福利-亚洲欧美日韩高清中文|