TaC?carbide has been?one of the earliest carbide?put into industrial production?since traditional WC-Co carbides can no longer meet people’s demands for higher product quality. TaC is considered to improve the high-temperature performance of carbide. Meetyou Hardmetal Corp. conducted the following experiment, using WC with different particle sizes as the research object, and studying the properties of TaC tungsten carbide?sintered at different temperatures.

Experiment method

The formulation of the carbide?consists of w(Co)=6.0% and w(TaC)=1.85%. In the WC powder, the mass fraction of particles with an average Fechner size of 4.90μm is 44%, and the mass fraction of particles with a size of 0.89μm is 56%.

The ball-to-powder ratio is 4:1, and the mixture is wet-milled in ethanol at a speed of 50r/min for 65 hours in a 160mm diameter ball mill. Then, the powder is pressed into a B-type bar with dimensions of 20mm x 5.4mm x 6.5mm using a rubber processing procedure. The bars are sintered in a vacuum dewaxing furnace at 1425℃, 1450℃, and 1500℃ for 1.5 hours each.

Afterwards, our experimental staff analyzed the microstructure of the material using scanning electron microscopy, measured its density using an analytical balance, measured its Vickers hardness using a Vickers hardness tester (HV30, with a pressure time of 15 seconds), measured its bending strength using a tensile testing machine, and measured its coercivity using a coercivity meter.

 

Experimental data on TaC carbide

The microstructure of the TaC carbide?material obtained is shown in Figure 1.

sample pic of TaC carbide

From Figure 2, it can be seen that at a sintering temperature of 1425°C, the grain size mainly distributed in ultra-fine grains, showing a normal distribution. At a sintering temperature of 1450°C, the grain size was concentrated in adjacent ultra-fine and ultra-submicron grains, accounting for nearly 70% of the total statistics. The number of nanocrystals also reached its highest value.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 2

At a sintering temperature of 1500°C, the grain size mainly distributed in ultra-fine grains, but some grains grew significantly, resulting in a decrease in the proportion of nanocrystals and ultra-submicron grains, and an increase in the proportion of medium-sized and coarse grains, resulting in a more scattered grain size distribution.

 

Experimental result analysis

The impact of sintering temperature on mechanical properties

The microstructure and properties of the TaC carbide material obtained are shown in Figure 2, where the bending strength and hardness of the sample increase with the increase of sintering temperature. Therefore, when sintered at 1500°C, the TaC carbide grain size continues to grow. From Figure 3, it can be seen that with the increase of sintering temperature, the bending strength value slightly increases.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 3

The bending strength of the carbide?increases as the uniformity of the WC average grain size improves. When the sample is sintered at 1450°C, the average grain size distribution is uniform, and the bending strength slightly increases. When sintered at 1500°C, the excessively high sintering temperature causes the WC grains to grow through the dissolution-precipitation process, and the increase in grain size is beneficial to improve the bending strength of the carbide. However, overall, the change in bending strength value from 914 MPa to 1081 MPa with the increase in temperature is not very significant.

 

 

The effect of sintering temperature on density and coercivity

Figure 4 shows the variation curves of density and coercivity of the samples with the change of sintering temperature. Density is one of the important physical properties of powder metallurgical materials, and the change of compact size during sintering is closely related to the change of density.

3 aspekty, które wp?ywaj? na temperatur? spiekania Tac Carbide 4

At 425 ℃ sintering, the shrinkage is incomplete and there are voids present, resulting in a lower density value. With the increase of sintering temperature, the flowability of the bonding phase improves, which is beneficial to eliminate pores and increase the density of the carbide.

When the temperature rises to 1,500 ℃, the volatilization of Co leads to a decrease in the amount of liquid phase, which is not conducive to pore filling, resulting in a decrease in density value.

 

As for coercivity, in WC-Co carbides, the coercivity is mainly related to the Co content and its dispersion. When non-magnetic η-phase appears in the carbide, the coercivity will increase due to the corresponding reduction in the amount of Co phase and the refinement of WC grains. In carbides with normal microstructure, as the carbon content decreases, the tungsten content in the Co phase increases, which strengthens the Co phase and increases the coercivity. At 1450 ℃ sintering, the grains of the sample are refined and evenly distributed, which maximizes the dispersion of the Co phase and thus maximizes the coercivity.

Wniosek

In this study, TaC?carbides were prepared using WC raw materials with different particle sizes and sintered at different temperatures. The following conclusions were drawn:

  1. Under the experimental conditions, the hardness, density, and coercivity of the carbideall first increase and then decrease with the temperature, and the sintering temperature has little effect on the bending strength of the carbide. When sintered at 1450 ℃ and held for 1.5 h, the comprehensive performance of the carbide?is the best, with a Vickers hardness (HV30) of 1668.8, a bending strength of 988 MPa, a density of 14.87 g/cm3, and a coercivity of 15.2 kA/m.
  2. When using mixed particle size WC, TaC has the best inhibitory effect on WC grain at 1450 ℃.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

日韩欧美国产综合久久-国产精品一起草在线观看| 亚洲欧美日韩国产一区二区三区-国产欧美日韩一区二区免费| 国产精品熟女视频一区二区-国产日韩精品欧美一区喷水| 欧美精品啪啪人妻一区二区-嫩草人妻舔舔羞羞一区二区三区| 国产免费一区二区三区不-日本少妇免费一区二区三区| 国产黄片在现免费观看-色老板最新在线播放一区二区三区| 亚洲欧美日韩国产一区二区三区-国产欧美日韩一区二区免费| 欧美日本亚一级二级三区久久精品-日韩欧美一区二区久久婷婷| 人妻互换精品一区二区-夜夜爽一区二区三区视频| 性色国产成人久久久精品二区三区-偷窥中国美女洗澡视频| 一级小黄片在线免费看-亚洲欧美午夜情伊人888| 国产精品一区二区在线免费-久久精品国产亚洲av热明星| 99久热精品免费观看四虎-亚洲天堂精品视频在线| 日韩欧美国产综合久久-国产精品一起草在线观看| 中文字幕日韩精品不卡一区二区-成人av在线观看一区二区| 中文字幕精品一区二区日本99-青青国产成人久久91网| 婷婷综合在线视频观看-亚洲一区二区三区香蕉| 精品亚洲卡一卡2卡三卡乱码-一区三区二插女人高潮在线观看| 欧美日韩黑人在线播放-51在线精品免费视频观看| 五月婷婷免费观看视频-男人操女人下面视频在线免费看| 中文字幕精品一区二区日本99-青青国产成人久久91网| 久久人妻一区二区三区欧美-国内不卡的一区二区三区| 91精品国产影片一区二区三区-欧美精品久久久精品一区二区| 丝袜美腿人妻连续中出-在线观看日韩三级视频| 白嫩美女娇喘呻吟高潮-久久一区二区三区日产精品| 久久久国产精品电影片-精品孕妇人妻一区二区三区| 三上悠亚免费观看在线-青青草原在线视频观看精品| 日韩亚洲一区二区三区av-欧美综合在线观看一区二区三区| 日韩高清在线观看一区二区-美产av在线免费观看| 国产欧美一区二区三区嗯嗯-欧美一区二区日本国产激情| 国产一区二区三区四区五区麻豆-欧美一级在线视频播放| 亚洲欧洲成视频免费观看-国产福利一区二区在线观看| 性都花花世界亚洲综合-日韩av一区二区三区| 精品少妇一区二区18-一区二区三区日韩在线播放| 亚洲av日韩五月天久热精品-国产日韩欧美一区二区三区群战| 免费av一区在线观看-国产精品视频高潮流白浆视频免费| av中文字幕男人天堂-懂色av一区二区三区在线观看| 国产av剧情护士麻豆-三级国产精品欧美在线观看| 欧美精品啪啪人妻一区二区-嫩草人妻舔舔羞羞一区二区三区| 成人av一区二区蜜桃-亚洲色图激情人妻欧美| 欧美视频在线观看国产专区-亚洲91精品在线观看|