TaC?carbide has been?one of the earliest carbide?put into industrial production?since traditional WC-Co carbides can no longer meet people’s demands for higher product quality. TaC is considered to improve the high-temperature performance of carbide. Meetyou Hardmetal Corp. conducted the following experiment, using WC with different particle sizes as the research object, and studying the properties of TaC tungsten carbide?sintered at different temperatures.

Experiment method

The formulation of the carbide?consists of w(Co)=6.0% and w(TaC)=1.85%. In the WC powder, the mass fraction of particles with an average Fechner size of 4.90μm is 44%, and the mass fraction of particles with a size of 0.89μm is 56%.

The ball-to-powder ratio is 4:1, and the mixture is wet-milled in ethanol at a speed of 50r/min for 65 hours in a 160mm diameter ball mill. Then, the powder is pressed into a B-type bar with dimensions of 20mm x 5.4mm x 6.5mm using a rubber processing procedure. The bars are sintered in a vacuum dewaxing furnace at 1425℃, 1450℃, and 1500℃ for 1.5 hours each.

Afterwards, our experimental staff analyzed the microstructure of the material using scanning electron microscopy, measured its density using an analytical balance, measured its Vickers hardness using a Vickers hardness tester (HV30, with a pressure time of 15 seconds), measured its bending strength using a tensile testing machine, and measured its coercivity using a coercivity meter.

 

Experimental data on TaC carbide

The microstructure of the TaC carbide?material obtained is shown in Figure 1.

sample pic of TaC carbide

From Figure 2, it can be seen that at a sintering temperature of 1425°C, the grain size mainly distributed in ultra-fine grains, showing a normal distribution. At a sintering temperature of 1450°C, the grain size was concentrated in adjacent ultra-fine and ultra-submicron grains, accounting for nearly 70% of the total statistics. The number of nanocrystals also reached its highest value.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 2

At a sintering temperature of 1500°C, the grain size mainly distributed in ultra-fine grains, but some grains grew significantly, resulting in a decrease in the proportion of nanocrystals and ultra-submicron grains, and an increase in the proportion of medium-sized and coarse grains, resulting in a more scattered grain size distribution.

 

Experimental result analysis

The impact of sintering temperature on mechanical properties

The microstructure and properties of the TaC carbide material obtained are shown in Figure 2, where the bending strength and hardness of the sample increase with the increase of sintering temperature. Therefore, when sintered at 1500°C, the TaC carbide grain size continues to grow. From Figure 3, it can be seen that with the increase of sintering temperature, the bending strength value slightly increases.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 3

The bending strength of the carbide?increases as the uniformity of the WC average grain size improves. When the sample is sintered at 1450°C, the average grain size distribution is uniform, and the bending strength slightly increases. When sintered at 1500°C, the excessively high sintering temperature causes the WC grains to grow through the dissolution-precipitation process, and the increase in grain size is beneficial to improve the bending strength of the carbide. However, overall, the change in bending strength value from 914 MPa to 1081 MPa with the increase in temperature is not very significant.

 

 

The effect of sintering temperature on density and coercivity

Figure 4 shows the variation curves of density and coercivity of the samples with the change of sintering temperature. Density is one of the important physical properties of powder metallurgical materials, and the change of compact size during sintering is closely related to the change of density.

3 aspekty, które wp?ywaj? na temperatur? spiekania Tac Carbide 4

At 425 ℃ sintering, the shrinkage is incomplete and there are voids present, resulting in a lower density value. With the increase of sintering temperature, the flowability of the bonding phase improves, which is beneficial to eliminate pores and increase the density of the carbide.

When the temperature rises to 1,500 ℃, the volatilization of Co leads to a decrease in the amount of liquid phase, which is not conducive to pore filling, resulting in a decrease in density value.

 

As for coercivity, in WC-Co carbides, the coercivity is mainly related to the Co content and its dispersion. When non-magnetic η-phase appears in the carbide, the coercivity will increase due to the corresponding reduction in the amount of Co phase and the refinement of WC grains. In carbides with normal microstructure, as the carbon content decreases, the tungsten content in the Co phase increases, which strengthens the Co phase and increases the coercivity. At 1450 ℃ sintering, the grains of the sample are refined and evenly distributed, which maximizes the dispersion of the Co phase and thus maximizes the coercivity.

Wniosek

In this study, TaC?carbides were prepared using WC raw materials with different particle sizes and sintered at different temperatures. The following conclusions were drawn:

  1. Under the experimental conditions, the hardness, density, and coercivity of the carbideall first increase and then decrease with the temperature, and the sintering temperature has little effect on the bending strength of the carbide. When sintered at 1450 ℃ and held for 1.5 h, the comprehensive performance of the carbide?is the best, with a Vickers hardness (HV30) of 1668.8, a bending strength of 988 MPa, a density of 14.87 g/cm3, and a coercivity of 15.2 kA/m.
  2. When using mixed particle size WC, TaC has the best inhibitory effect on WC grain at 1450 ℃.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

91蜜桃传媒一二三区-日韩欧美国产一区呦呦| 欧美日韩国产在线资源-超碰成人国产一区二区三区| 亚洲国产视频不卡一区-激情欧美视频一区二区| av网址在线直接观看-黄色av全部在线观看| 国产精品久久久精品一区-99久久免费精品国产男女性高好| 91大神国内精品免费网站-亚洲免费电影一区二区| 欧美一级二级三级在线看-日韩精品欧美嫩草久久99| 97人妻精品一区二区三区爱与-日韩精品亚洲专区在线观看| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 中文字幕亚洲中文字幕-丰满老妇伦子交尾在线播放| 亚洲美女喘息呻吟的网站-国产免费一区二区三区三洲| 日韩精品中文在线观看一区-亚洲bt欧美bt精品| 亚洲女人黄色录像一区-日韩av电影在线免费看| 国产成人精品亚洲精品密奴-国产成人AV无码精品| 一区二区三区国产高清mm-美女张开腿让帅哥桶爽| 欧美精品国产系列一二三国产真人-在线观看国产午夜视频| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 成人av一区二区蜜桃-亚洲色图激情人妻欧美| 黄色av网站在线免费观看-亚洲欧美精品偷拍tv| 精品亚洲卡一卡2卡三卡乱码-一区三区二插女人高潮在线观看| 俄罗斯胖老太太黄色特级片-国产精品黑丝美腿美臀| 亚洲国产精品一区二区av-日本一级黄色一区二区| 精品国产综合一区二区三区-蜜臀一区二区三区刺激视频| 乱入一二三免费在线观看-久久精品亚洲精品国产色婷婷| 久久久国产精品电影片-精品孕妇人妻一区二区三区| 欧美日韩国产综合新一区-国产综合av一区二区三区| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 99久久精品一区二区成人-麻豆国产av玩弄放荡人妇系列| 亚洲黑人欧美一区二区三区-亚洲一区二区三区免费视频播放| 亚洲另类自拍唯美另类-99国产精品兔免久久| 国产午夜精品理论片A级漫画-久久精品国产99亚洲精品| 日本少妇激情一区二区-亚洲自偷自拍熟女另类蜜臀| 婷婷亚洲欧美综合丁香亚洲-超刺激国语对白在线视频| 亚洲av专区在线观看国产-丰满人妻av一区二区三区| 亚洲愉拍自拍欧美精品app-亚洲一区不卡在线视频| 久艹在线观看视频免费-人妻偷人精品一区二区三区| 国产欧美日韩中文字幕在线-国产伊人一区二区三区四区| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 日韩国产一区二区三区在线-精品日韩人妻少妇av| 欧美一级一线在线观看-亚洲一区二区亚洲三区| 99热在线精品免费6-av一区二区在线观看|