Wet milling can grind hard phases (mainly WC phase) to the required particle size and achieve a uniform mixing state with Co powder in a small range, which has good compaction and sintering properties. Therefore, the wet milling time is also one of the key parameters in the preparation process of hard alloys. This article mainly studies the influence of wet milling time on the microstructure and properties of hard alloys.

Experimental materials for wet milling and methods

The recycled WC-Co composite powder produced by zinc melting method was used as the experimental material, and its composition is shown in Table 1.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci YG8 (ISO K30) W?glik spiekany 2

Laser particle size analysis showed that the median diameter was 3.46μm, with a narrow range of particle size distribution and relatively concentrated particle size. Figure 1 shows the SEM image of the original morphology of the WC-Co composite powder.

Effects of Wet?milling Time on Microstructure and Properties of YG8(ISO K30) Cemented Carbide 3

From Fig.1, it is evident that the recycled powder has mild agglomeration, and its morphology is mostly triangular or rectangular with smooth edges, retaining the characteristics of WC grains in hard alloys. The average particle size of the powder is about 3μm, which is consistent with the results obtained from laser particle size analysis.

 

Figure 2 shows the XRD spectrum of the WC-Co composite powder.

Effects of Wet?milling Time on Microstructure and Properties of YG8(ISO K30) Cemented Carbide 4

Experimental Results and Discussion about wet milling time

Figure 3 shows the morphology of WC-Co composite powders after different wet milling?times. As shown in Figure 3(a), when wet milling?for 18 hours, the powder size is relatively large and unevenly distributed, indicating that the wet milling?effect is not ideal, and the collision between the grinding balls and the powder in the tank is insufficient, and the powder refinement is not enough. After wet milling?for 24 hours (Figure 3(b)), it was found that the powder size decreased rapidly, and the refinement was obvious, but the uniformity was limited. It can be observed that the powder fragmentation mainly occurred due to the repeated impact and friction of the grinding balls, resulting in the rupture of large particles into smaller particles. Continuing wet milling?until 30 hours (Figure 3(c)), it can be found that there is not much change in the powder size, but the uniformity and morphology have improved, with an average particle size between 1 and 2 μm. This indicates that the powder wet ground for 30 hours has a relatively ideal particle size and morphology. Apart from the rupture, the powder is mainly worn out (WC corners are worn out, producing fine powder). Finally, after wet milling?for 36 hours, it is evident that the powder not only did not refine further but also showed agglomeration phenomenon B (see Figure 3(d)).

wet milling time

 

It should be noted that the powder cannot be infinitely refined during ball milling. During ball milling, as the particle size of the powder decreases, the specific surface area of the powder increases exponentially, exhibiting high surface energy and a sharp increase in reactivity, making it easy to agglomerate and bond with other powders to resist the increase in total energy. As a result, on the one hand, external energy is input into the powder, causing it to refine; on the other hand, the powder agglomerates and forms lumps, reducing the system energy. After the combined effect of these two trends, a dynamic equilibrium is reached between them, and the average particle size of the powder will eventually stabilize within a certain range. In this experiment, the powder was ball milled for 30 hours, and its uniformity was good, with a particle size reaching an equilibrium value (1-2 μm).

Figure 4 shows the XRD patterns of sintered regenerated cemented carbide with different wet milling times. As shown in the figure, when wet milled for 18 hours, the alloy contains impurity phase of elemental carbon (C); as wet milling continues, the elemental carbon disappears. This indicates that the alloy is slightly carburized during wet milling for 18 hours, and as the wet milling time is prolonged, the powder is refined and the surface adsorbs more oxygen, resulting in an increase in the oxygen content of the mixture. During sintering, part of the carbon is consumed, resulting in the formation of a pure two-phase structure of WC and Co in the alloy, and no other impurity phases were found.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci w?glika spiekanego YG8 (ISO K30) 5

Figure 5 shows the metallographic images of the cemented carbide after corrosion for different wet milling times. Comparing Figures 5 (a) to (d), it can be seen that under the sintering process (1723 K, pressure), the alloy structure is good, and no defects such as abnormally large WC grains and cobalt pools were found. The grain size of the alloy is slightly smaller with a polygonal morphology after wet milling for 24 hours compared to 18 hours, and the Co phase is evenly distributed. As wet milling continues, there is no significant change in grain size, but the uniformity slightly improves. When wet milled for 36 hours, it was found that the WC grains had slightly grown, which may be related to the partial agglomeration of the powder during wet milling.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci w?glika spiekanego YG8 (ISO K30) 6

It is worth noting that as the wet milling?time increases, the strength of the alloy shows a continuous upward trend, but the magnitude of the increase becomes smaller and smaller. Generally, for the same Co content and without obvious defects, the strength of the alloy is related to the distribution of internal micro-pores and WC grain size. When wet milling?for 18 hours, due to the short time, the material mixing is uneven, the powder refinement degree is insufficient, the particle size is large, and the distribution is uneven, resulting in the easy formation of micro-pores during sintering, thus the alloy strength is not high. Continuing wet milling?further breaks down the powder particles, increases the number of fine WC particles, narrows the WC particle size distribution towards homogenization, and eliminates the coarse WC grains, which are the main sources of cracks, resulting in an increase in the bending strength of the alloy.

In WC-Co alloys with the same Co content, the coercive force of the alloy is inversely proportional to the WC grain size and distribution, which is consistent with the description in Figure 5.

Wp?yw czasu mielenia na mokro na mikrostruktur? i w?a?ciwo?ci w?glika spiekanego YG8 (ISO K30) 7

Figure 6 shows the distribution of flexural strength for regenerated cemented carbides with different wet milling times. Based on Figure 6, the range of strength values for each alloy can be observed, which gives the variation of the strength of the statistical samples. It can be seen from the figure that there are many overlaps and dispersions in the experimental results. It is easy to find that with the extension of wet milling time, not only the strength of the alloy increases, but also the fluctuation range becomes narrower, and each strength value is closer to each other. This indicates that the extension of wet milling time can reduce the discreteness of the strength distribution of regenerated cemented carbides.

 

Wniosek

Under the experimental conditions of this study, the effects of different wet milling?times on the microstructure and properties of recycled WC-8Co composite powder and sintered hard alloys were investigated, and the following conclusions were drawn:

  1. Continuous wet millingfor 30 hours with a ball-to-powder ratio of 3:1 resulted in fine and uniformly distributed composite powder with an average particle size of 1-2 μm, as observed by SEM.
  2. Under the conditions of continuous wet millingfor 36 hours with a ball-to-powder ratio of 3:1 and sintering process (1723 K for 1 hour with a pressure of 5 MPa), the alloy exhibited the best comprehensive properties. Its density was 14.71 g/cm3, HRA90.1, the average strength was 3560 MPa, cobalt magnetism was 7.2%, and coercivity was 15.8 kA/m.
  3. The analysis of the strength distribution of alloys with different wet millingtimes showed that within a certain range, the prolongation of wet milling?time can reduce the discreteness of the strength distribution of recycled hard alloys.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

国产精品久久99精品毛片-国产四季高清一区二区三区| 国产在线不卡高清一区-日本一区二区三区四区无卡| 久久精品亚洲国产av久-国产精品视频一区二区免费| 99精品只有久久精品免费-蜜臀一区二区三区精品久久久| 日韩av电影一区二区网址-老熟妇仑乱视频一区二| 九九热这里只有精品九九-欧美日韩人妻精品一二三| 精品国产综合一区二区三区-蜜臀一区二区三区刺激视频| 国语自产偷拍精品视频偷拍-国产伊人这里只有精品视频| 少妇人妻无码久久久久久-综合图片亚洲网友自拍| 久久久噜噜噜久久狠狠50岁-精品一区二区三区av| 三级a级一级大片在线观看-日韩av有码免费观看| 亚洲美女喘息呻吟的网站-国产免费一区二区三区三洲| 国产成人精品免费视频大全办公室-亚洲欧美日本综合在线| av噜噜国产在线观看-欧美视频亚洲视频一区二区三区| 国产在线观看高清精品-四季av一区二区三区中文字幕| 久久网站中文字幕精品-三级精品久久中文字幕| 亚洲欧美另类综合偷拍-婷婷社区综合在线观看| 99精品只有久久精品免费-蜜臀一区二区三区精品久久久| 欧美亚洲另类久久久精品-国产精品一区二区亚洲推荐| 97人妻精品一区二区三区爱与-日韩精品亚洲专区在线观看| 18禁真人在线无遮挡羞免费-中文字幕精品一区二区三区四区| 国产人妻人伦精品日本-国产98超碰人人做人人爱| 天天干天天日天天射天天舔-精品香蕉视频官网在线观看| 欧美三级韩国三级日本三斤-日本不卡一区不卡二区| 国产综合日韩激情在线-日韩精品人妻一专区二区三区| 人妻互换精品一区二区-夜夜爽一区二区三区视频| 色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 91蜜桃传媒一二三区-日韩欧美国产一区呦呦| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 久久蜜桃精品一区二区-麻豆视频啊啊啊好舒服| 91大神国内精品免费网站-亚洲免费电影一区二区| 国产精品电影在线一区-亚洲国产大片一区二区官网| 国产一区二区三区噜噜-精品久久亚洲一区二区欧美| 亚洲国产精品一区二区av-日本一级黄色一区二区| 久久影视av一区二区-人妻激情乱偷一区二区三区| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 国产成人精品亚洲精品密奴-国产成人AV无码精品| 日韩亚洲欧美综合在线-成人在线网站在线观看| 亚洲最新国产无人区123-黄片一区二区在线观看| 国产人妻人伦精品日本-国产98超碰人人做人人爱|