In recent years, the production technology of ultra-fine grain cemented carbide has developed rapidly, especially in the key technology of preparing ultra-fine grain WC powder, where the competition is very fierce. Many promising methods have emerged, some of which have reached the level of practical application. However, there are few reports in domestic literature, especially on basic theories or regularity research. In the process of developing the preparation technology of ultra-fine grain WC powder, this paper deeply investigates the influence of the particle size of carbon black powder on the carbon content of WC powder under different carbonization temperatures when using ultra-fine (0.35 μm) tungsten powder.

 

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 2

Experimental Content and Method

Test Materials of WC powder

(1) Ultra-fine tungsten powder: The ultra-fine tungsten powder is prepared by the ultrasonic spray pyrolysis method from ultra-fine WO? powder, which is generally amorphous with an average particle size of 25~30 nm. It is reduced by hydrogen at a medium temperature (750~780℃) to obtain tungsten powder with an average particle size of ≤0.35μm (BET particle size).

(2) Carbon black powder: Carbon black powder is produced by two methods: one is by cracking ethane and propane (at 850℃) and then subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.1 and 0.3 μm, respectively; the other is from activated carbon powder with an original particle size of 100~200μm, which is subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.8 and 4.5 μm, respectively.

Experimental Method

Using ultra-fine tungsten powder with the same particle size (0.35 μm) and four different particle sizes (0.1, 0.3, 0.8, 4.5 μm) of carbon black powder, the carbon is blended according to the reaction formula W+C=WC (with an additional loss of 0.1%). The mixture is ball milled for 1.5 hours in a conventional ball mill with a ball-to-material ratio of 1:1. The heat-resistant stainless steel boat containing the mixed material is placed in a stainless steel tube furnace and carbonized under a hydrogen atmosphere. The holding time is 40 minutes for all. In the temperature range of 830~1300℃, the carbonized material is taken out at different temperatures, cooled, and then removed from the furnace. Subsequently, XRD phase analysis and chemical analysis are conducted to determine the total carbon and free carbon, and the amount of combined carbon in WC is calculated. Finally, the quantitative relationship between the particle size of carbon black powder and the phase composition and combined carbon content of WC powder under different carbonization temperatures can be plotted.

 

Test Results and Discussion

Figure 1 shows the effect of carbon black powder with different particle sizes carbonized at different temperatures on the combined carbon content of WC powder. Curve 1 in Figure 1 represents the relationship between carbonization temperature and the combined carbon content of WC powder when using ultra-fine carbon black powder with a particle size of 0.1 μm. As can be seen from Figure 1, when using 0.1 μm ultra-fine carbon black, the combined carbon content of WC powder can reach 5.8% (by mass), which is equivalent to 95% of the theoretical content, at a very low carbonization temperature (850℃). When the temperature is greater than 950℃, the carbon content of WC powder can reach the theoretical content. This result indicates that the carbonization reaction can be completed at a low temperature when using ultra-fine tungsten powder in conjunction with ultra-fine carbon black powder. This phenomenon suggests that the ultra-fine W powder particles are carbonized before they undergo significant aggregation and growth.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 3
At this temperature, as the particle size of the carbon black used increases, the combined carbon content in WC powder rapidly decreases. For example, as shown in Curve 2 of Figure 1, when using 0.3 μm carbon black at 950℃ with the same holding time of 40 minutes, the combined carbon content of WC powder only reaches 5.2% (by mass). XRD analysis indicates that there is still significant W?C in the WC powder, as shown in Figure 2. The free carbon phase was not detected due to its low content. The combined carbon content in WC powder can only reach the theoretical value when the temperature is increased to 1060℃. Its complete carbonization temperature is about 130℃ higher than that of the 0.1 μm carbon black.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 4

When using 0.8 μm carbon black, as shown in Curve 3 of Figure 1, at 950℃ with a holding time of 40 minutes, the combined carbon content of WC is only 3.18% (by mass). XRD analysis indicates that in addition to the obvious W?C phase, there is also significant free carbon present in the WC powder, as shown in Figure 3. The combined carbon content in WC powder can only reach the theoretical value when the carbonization temperature is increased to 1230℃. The temperature required for complete carbonization has increased significantly.
The reason for this phenomenon is that when the carbon content ratio is constant, the finer the carbon black particle size, the easier it is to mix uniformly with W powder particles, increasing the contact area between them. Undoubtedly, fine-grained carbon black will accelerate the carbonization rate. Moreover, the finer the carbon black particle size, the more its specific surface area and the number of active carbon atoms on the surface increase dramatically. Thus, the carbonization reaction rate between carbon and tungsten accelerates, and the complete carbonization temperature decreases with the decrease of carbon black particle size.

WC powder

Conclusions

(1) When the particle size of ultra-fine W powder is the same (≤0.35μm), the combined carbon content in WC powder decreases significantly with the increase of the carbon black particle size at a certain temperature.
(2) When the particle size of carbon black is constant, the content of combined carbon increases with the rise of carbonization temperature.

Leave a Reply

Your email address will not be published. Required fields are marked *

久久网站中文字幕精品-三级精品久久中文字幕| 国产欧美日韩精品一区在线-久久精品视频免费获取地址| 日韩综合精品一区二区-丝袜美腿熟女人妻经典三级| 欧美日韩国产亚洲免费-肉体粗喘娇吟国产91| 国产一级片久久免费看同-麻豆精品尤物一区二区青青| 久久免费观看归女高潮特黄-黄色av一本二本在线观看| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 一区二区三区女同性恋-熟妇高潮一区二区高清网络视频| 色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 青青操视频在线观看国产-欧美成人乱码在线观看| 久久夜色精品亚洲噜国产av-大香蕉伊人猫咪在线观看| 久艹在线观看视频免费-人妻偷人精品一区二区三区| 99久久精品一区二区成人-麻豆国产av玩弄放荡人妇系列| 成人免费黄色在线网站-日韩精品一区二区三区四区在线| 四虎成人在线免费视频-亚洲熟女中文字幕天堂| 欧美日韩黑人在线播放-51在线精品免费视频观看| 国产福利视频一区二区三区-日韩人妻中文视频精品| 日本韩国亚洲欧美三级-日本东京不卡网一区二区三区| 黄色av网站在线免费观看-亚洲欧美精品偷拍tv| 国产美女网站在线观看-国产精品亚洲综合网69| 国产欧美成人精品第一区-日本黄色精品一区二区| 亚洲一区二区少妇激情-国产精品美女久久高潮| 欧美aa一级视频播放-久一一区二区三区大香蕉| 在线免费观看黄片喷水-国产精品白丝网站在线观看| 久久久国产精品电影片-精品孕妇人妻一区二区三区| 亚洲产国偷v产偷v自拍性色av-亚洲欧美日韩国产三区| av网址在线直接观看-黄色av全部在线观看| 男人的天堂久久精品激情-最新亚洲精品a国产播放| 午夜福利卫生纸福利院-一区二区三区久久亚洲| 欧美一级一线在线观看-亚洲一区二区亚洲三区| 欧美日韩黑人在线播放-51在线精品免费视频观看| 性都花花世界亚洲综合-日韩av一区二区三区| 亚洲国产中文欧美一区二区三区-国产精品一区二区视频成人| 亚洲av日韩五月天久热精品-国产日韩欧美一区二区三区群战| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 天天日天天干天天综合-99久久综合狠狠综合久久| 一区二区国产高清在线-日本高清无卡一区二区三区| 天天日天天干天天综合-99久久综合狠狠综合久久| 四虎成人在线免费视频-亚洲熟女中文字幕天堂| 久久特一级av黄色片-91社区视频免费观看| 国产在线不卡高清一区-日本一区二区三区四区无卡|