Machining titanium alloy is hard because the thermal conductivity of titanium alloy is very poor. Coupled with the short contact length between the chip and the cutting tool, it is not conducive to the dissipation of cutting heat. As a result, the temperature in the cutting edge region is high, about more than twice that of cutting 45 steel. In addition, tool wear is also severe. On the one hand, the strong chemical affinity between titanium alloy and tool material makes it easy to bond with elements such as Ti, Co, and C in the tool material, aggravating adhesive wear at high temperatures. On the other hand, titanium alloy easily forms a hard and brittle surface layer by reacting with oxygen and nitrogen in the air, exacerbating tool wear.

Table 1: Selection of Tool Geometric Parameters for Turning Titanium Alloys

Tool material Front Rake Angle ?Back Rake Angle Cutting Edge Inclination Angle Main Clearance Angle Secondary Clearance Angle Chamfer Width (mm) Chamfer Front Angle Cutting Edge Radius (mm)
Carbide lathe 5~10 10~15 0~10 45~75 15 0.05~0.3 0.10~0 0.5~1.5

What are the Challenges in Machining Titanium Alloys? 1

Machining amount

The cutting speed for turning titanium alloys should not be too high, and the cutting depth can be relatively large, while the feed rate should be appropriate. A feed rate that is too large can cause burning of the cutting edge, while a feed rate that is too small results in rapid wear of the cutting edge when processing the hardened layer. When turning titanium alloys, rust-proof emulsion or extreme-pressure emulsion can be used for cooling and lubrication. The recommended cutting parameters for turning titanium alloys are as shown in

Table 2: Selection of Cutting Parameters for Turning Titanium Alloys

Feed (mm) cutting speed(mm)
0.08~0.12 87~69
0.13~0.17 71~59
0.16~0.24 62~51
0.25~0.30 53~47
0.33~0.44 48~41
0.45~0.65 42~34

Note: Conditions for the use of this table: Tool material YG8, workpiece material TC4, tool geometric angles front rake angle = 5°, back rake angle = 10°, main clearance angle = 75°, secondary clearance angle = 15°, cutting edge radius = 0.5mm, turning depth = 1mm, dry turning. If using cutting fluid, the turning speed in the table can be appropriately increased.

What are the Challenges in Machining Titanium Alloys? 2

Machining parameters

Machining Temp.

When turning titanium alloys, the cutting temperature is high, and tool durability is low. Among the cutting parameters, cutting speed has the most significant impact on cutting temperature. Therefore, efforts should be made to ensure that the cutting temperature generated at the selected cutting speed is within the optimal range. The recommended cutting temperature for turning titanium alloys with high-speed steel tools is approximately 480°C to 540°C, while for hard alloy tools, it is around 650°C to 750°C.

Cutting speed Vc

The cutting speed has the most significant impact on tool durability, and it is preferable to operate the tool at the optimal cutting speed with minimal relative wear. When turning titanium alloys of different grades, the cutting speed should be adjusted appropriately due to significant differences in strength. The turning depth also has a certain influence on the cutting speed, and the magnitude of the cutting speed should be determined based on different turning depths.

Feed rate

The feed rate has a relatively small impact on tool durability. While ensuring the machining surface roughness, a larger feed rate can be chosen, typically ranging from f=0.1 to 0.3 mm/r. If the feed rate is too small, the tool may cut within the hardened layer, increasing tool wear. Additionally, extremely thin chips are prone to spontaneous combustion at high cutting temperatures, so a feed rate below f<0.05 mm/r is not allowed.

Cutting depth (ap) has the least impact on tool durability. A larger cutting depth is generally chosen to avoid cutting within the hardened layer, reducing tool wear. It also increases the working length of the cutting edge, promoting heat dissipation. Typically, ap is set at 1 to 5 mm.

Leave a Reply

Your email address will not be published. Required fields are marked *

久久蜜桃精品一区二区-麻豆视频啊啊啊好舒服| 黄色91av免费在线观看-欧美黄片一级在线观看| 亚洲视频一区二区三区免费-国产一级黄色大片在线| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 婷婷人妻少妇激情在线-欧美日韩人体艺术一区二区| 极品人妻av在线播放-久久精品视频一区二区三区| 日韩亚洲欧美综合在线-成人在线网站在线观看| 青青操视频在线观看国产-欧美成人乱码在线观看| 久久影视av一区二区-人妻激情乱偷一区二区三区| 国产av一区二区三区日韩接吻-av网址在线播放网站| 97一区二区三区在线-欧美护士性极品hd4k| 天天干天天天天天天天-亚洲综合av在线三区| 亚洲日本一区二区三区黄色电形-中文字幕乱码免费熟女| 成人免费黄色在线网站-日韩精品一区二区三区四区在线| 青木玲高清中文字幕在线看-视频在线免费观看你懂的| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 亚洲日本一区二区三区黄色电形-中文字幕乱码免费熟女| 欧美日韩亚洲1区2区-黄污视频在线观看不卡| 亚洲欧美日韩二区三区-国产在线欧美一区日韩二区| 18禁真人在线无遮挡羞免费-中文字幕精品一区二区三区四区| 丝袜高跟熟女视频国产-熟女少妇亚洲一区二区| 亚洲国产精品一区二区av-日本一级黄色一区二区| 青青草原免费国产在线视频-精品人妻乱码一区二区三区四区| 亚洲愉拍自拍欧美精品app-亚洲一区不卡在线视频| 亚洲永久免费在线观看-亚洲欧美导航一区二区导航| 在线视频成人一区二区-亚洲另类中文字幕在线| 国产精品一区二区欧美视频-国产一区二区三区天码| 人妻互换精品一区二区-夜夜爽一区二区三区视频| 久久99国产综合精品女人-日韩一区二区三区在线不卡| 国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 日本中文字幕永久在线人妻蜜臀-欧美一区二区的网站在线观看| 国产精品成人欧美激情-黄色床上完整版高清无遮挡| 国产午夜精品理论片A级漫画-久久精品国产99亚洲精品| 国产在线观看高清精品-四季av一区二区三区中文字幕| 91大神国内精品免费网站-亚洲免费电影一区二区| mm在线精品视频在线观看-欧美国产日韩在线一区二区三区| 亚洲最新国产无人区123-黄片一区二区在线观看| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 久久蜜桃精品一区二区-麻豆视频啊啊啊好舒服| 成人免费黄色在线网站-日韩精品一区二区三区四区在线| 国产福利视频一区二区三区-日韩人妻中文视频精品|