Many structures made of WC-Co carbide are subject to thermo-mechanical loading and have to conduct heat in order to function properly in industrial application. The current work provides results on a significant drop in thermal conductivity of WC-Co carbides as a function of material volume damage that accumulates during cyclic high-temperature loading of the materials depending on material microstructure. Average WC grain size and Co binder metal content of the investigated grades ranged from submicron to medium and from 10 to 12 wt%, respectively. The carbides were subjected to uniaxial cyclic loading in a vacuum for different numbers of load cycles at 700 °C and 800 °C. Damage features accumulated in the material volume were documented by means of scanning electron microscopy. Thermal conductivity properties of virgin and damaged materials were determined via laser flash analysis. The results indicated a significant decrease depending on the materials’ microstructure, i.e. the defects’ predominant location within the microstructure. The damage features that occurred mainly between WC grains in the coarser-grained grade led to larger drops in thermal conductivity with rising temperature compared to damage features that occurred within the Co binder metal in the finer-grained grade. The presented results are of high relevance to the thermo-mechanical load situation of e.g. milling tools since the heat conduction away from their cutting edges is hindered by the documented effect and deemed to lead to a self-acceleration of the damage accumulation.

Study on the Properties of Spherical Cast Tungsten Carbide Powders Prepared by Different Methods 2

Spherical cast tungsten carbide powder is a new type of ultra-wear-resistant ceramic particle material. Compared with traditional tungsten carbide, spherical cast tungsten carbide has two significant advantages: first, it has a regular spherical appearance, good powder flowability, and wettability, which results in good integration with the surrounding tissue when added as particles, reducing the likelihood of stress concentration; second, the internal structure of the tungsten carbide particles is dense, with good toughness, fine grains, high hardness, and the coating has excellent wear resistance and is less likely to break under load. Due to its outstanding performance, spherical cast tungsten carbide powder is gradually replacing traditional tungsten carbide powder in the surface protection of components in mining machinery, oil machinery, construction industry, and foundries, significantly improving the wear resistance, corrosion resistance, and oxidation resistance of workpieces, and extending the service life of workpieces.

Introduction to the Methods of Spherical Cast Tungsten Carbide

Currently, the spherical cast tungsten carbide powders available in the market are mainly prepared by the following methods: induction remelting spheroidization, plasma remelting spheroidization, and plasma rotating electrode atomization.

The induction remelting spheroidization method involves heating the material in a reactor to the spheroidization temperature through induction heating, and the material moves forward slowly the vibration of the furnace tube. If the dispersion of the material is not well controlled, the molten droplets will grow due to collision and adhesion, making particle size control difficult. Moreover, during the operation, the powder must not come into contact with the reactor, otherwise it will affect the entire spheroidization process and cause material waste.

The plasma remelting spheroidization method uses casting tungsten carbide powder as the raw material and employs radiofrequency plasma flame to heat argon gas to a high temperature of 3000 to 10000 ℃, melting the casting tungsten carbide particles into a liquid state and directly quickly condensing them into spherical particles. This method can easily obtain fine-grained spherical tungsten carbide powder by controlling the particle size and composition of the raw material.

The plasma rotating electrode atomization method uses a tungsten carbide rod as the electrode, fixed within the rod material bin, and then subjected to plasma atomization under inert gas protection. The plasma arc melts the end face of the high-speed rotating rod, and under the action of centrifugal force, the molten droplets separate from the edge of the molten pool and solidify in the form of spherical particles. This technology avoids the difficulty of material dispersion at ultra-high temperatures during remelting spheroidization, and the obtained spherical tungsten carbide powder has a narrow particle size distribution range and is easy to control.

The following will study the chemical composition, micro-morphology, microstructure, microhardness, and other powder properties of spherical cast tungsten carbide powders prepared by different methods.

Study on the Properties of Spherical Cast Tungsten Carbide Powders Prepared by Different Methods 3

Chemical composition

Study on the Properties of Spherical Cast Tungsten Carbide Powders Prepared by Different Methods 4

The table above shows the chemical composition of spherical cast ??? ???? powder samples prepared by different methods. It can be observed that the main components of the spherical cast tungsten carbide powder are W and C elements, and all contain trace amounts of Fe, V, Cr, and Nb elements. The ideal spherical cast tungsten carbide should be a eutectic of WC and W2C, with an eutectic temperature of 2525 ℃ and a carbon content of 3.840% (by mass) at the eutectic point. From the data in the table, it can be seen that the total carbon content of the spherical cast tungsten carbide prepared by the plasma rotating electrode atomization method has the smallest deviation from the theoretical eutectic carbon content, with the lowest free carbon content; the powder obtained by the induction remelting spheroidization method has the largest difference in total carbon content from the theoretical value, with a difference of 0.170% (by mass). This is due to the carbon content increase caused by the graphite tube heating method used in the induction remelting spheroidization process. In addition, by comparing samples 2#, 3#, and 4# with similar particle sizes, it can be determined that the powder prepared by the plasma rotating electrode atomization method has the relatively lowest impurity content. However, the impurity content of sample 1# prepared by the plasma rotating electrode atomization method is relatively high, which may be related to the quality of the cast tungsten carbide raw material rod. This suggests that, compared to other methods, the plasma rotating electrode atomization method can more accurately control the carbon content of spherical cast tungsten carbide powder, preventing overeutectic and hypoeutectic reactions caused by carburization and decarburization, and obtaining a nearly complete eutectic structure, which is crucial for improving the microstructure and properties of spherical cast tungsten carbide.

 

??? ??

The Microscopic Morphology of Spherical Cast Tungsten Carbide Powder Samples
The Microscopic Morphology of Spherical Cast Tungsten Carbide Powder Samples

The image above shows the microscopic morphology of spherical cast tungsten carbide powders prepared by different methods. It can be observed that the spherical cast tungsten carbide powders prepared by the three methods are all regular and smooth, nearly spherical in shape.

Cross-sectional Photos of Spherical Cast Tungsten Carbide Powder
Cross-sectional Photos of Spherical Cast Tungsten Carbide Powder

The image above shows the cross-sectional photos of spherical cast tungsten carbide powders prepared by different methods. As can be seen from (a) and (b), the spherical tungsten carbide powder particles prepared by the plasma rotating electrode atomization method are dense with almost no defects. However, as seen in (c) and (d), there are some obvious pores within the spherical tungsten carbide powder particles prepared by the plasma remelting spheroidization method and the induction remelting spheroidization method, resulting in some hollow powders. The main reason for this is that the crushed tungsten carbide powder material used in the above methods is likely to contain residual pores from the casting process. During the short plasma or induction heating process, the interior of the crushed tungsten carbide powder is difficult to completely melt, leading to some residual pores within the particles.

????

Microstructure Photos of Spherical Cast Tungsten Carbide Powder Samples After Corrosion
Microstructure Photos of Spherical Cast Tungsten Carbide Powder Samples After Corrosion

The image above shows the microstructure photos of spherical cast tungsten carbide powder particles after corrosion. It can be observed that the internal structure of the spherical tungsten carbide powder particles prepared by the three methods mainly consists of a typical fine acicular WC and W2C eutectic structure. Compared to the plasma remelting spheroidization method and the induction remelting spheroidization method, the spherical cast tungsten carbide powder prepared by the plasma rotating electrode atomization method has a denser eutectic structure. This is because, unlike the plasma remelting spheroidization method and the induction remelting spheroidization method, the plasma rotating electrode atomization method completely melts the cast tungsten carbide feedstock rod and then solidifies by being thrown out under the action of centrifugal force. During the crystallization of the molten cast tungsten carbide, the degree of undercooling is greater, nucleation is more rapid, and a larger number of crystal nuclei are generated, resulting in a finer and denser eutectic structure.

 

???? ??

The table below shows the average microhardness of spherical cast tungsten carbide powders prepared by different methods. It can be seen that the microhardness of the spherical cast tungsten carbide powders prepared by the three methods is all above 2800 HV0.1, with the powder prepared by the plasma rotating electrode atomization method having the highest microhardness, reaching 3045 HV0.1. This is mainly due to the finer eutectic structure within the spherical cast tungsten carbide prepared by the plasma rotating electrode atomization method.

Other Physical Properties of spherical cast tungsten carbide

The table below shows the flowability and apparent density values of spherical cast tungsten carbide powders prepared by different methods. It can be seen that the powder prepared by the plasma rotating electrode atomization method has the worst flowability and the smallest apparent density; whereas the powder prepared by the induction remelting spheroidization method has the best flowability and the largest apparent density.

Study on the Properties of Spherical Cast Tungsten Carbide Powders Prepared by Different Methods 5

??

(1) The spherical cast tungsten carbide prepared by the plasma rotating electrode atomization method has the smallest deviation from the theoretical eutectic carbon content, the lowest free carbon content, and relatively low impurity content.

(2) The spherical tungsten carbide powder particles prepared by the plasma rotating electrode atomization method are dense with almost no defects, and the eutectic structure is finer. The spherical tungsten carbide powder particles prepared by the plasma remelting spheroidization method and the induction remelting spheroidization method both have some obvious pores, resulting in some hollow powders.

(3) The spherical cast tungsten carbide powders prepared by the three methods mainly consist of WC and W2C phases.

(4) The microhardness of the spherical cast tungsten carbide powders prepared by the three methods is all above 2800 HV0.1, with the powder prepared by the plasma rotating electrode atomization method having the highest microhardness, reaching 3045 HV0.1. The powder prepared by the induction remelting spheroidization method has the best flowability and the largest apparent density.

?? ???

???? ???? ????. ?? ???? * ? ???? ????

国产精品成人欧美激情-黄色床上完整版高清无遮挡| 亚洲国产精品一区二区av-日本一级黄色一区二区| 五月婷婷免费观看视频-男人操女人下面视频在线免费看| 韩漫一区二区在线观看-精品国产免费未成女一区二区三区| 午夜精品午夜福利在线-内射无套内射国产精品视频| 国产精品熟女视频一区二区-国产日韩精品欧美一区喷水| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 一区二区国产高清在线-日本高清无卡一区二区三区| 国产精品久久久精品一区-99久久免费精品国产男女性高好| 亚洲av高清一区三区三区-久久人妻夜夜做天天爽| 激情字幕久久久字幕中文-一区二区三区免费黄片| 熟女熟妇伦51788-国产av在线播放一区二区三区| 国产在线观看高清精品-四季av一区二区三区中文字幕| 婷婷六月视频在线观看-久久亚洲综合国产精品| 日韩精品亚洲不卡一区二区-成人网在线视频精品一区二区三区| 日本韩国亚洲欧美三级-日本东京不卡网一区二区三区| 五月婷婷六月在线观看视频-亚洲黑寡妇黄色一级片| 亚洲国产日韩精品四区-dy888午夜福利精品国产97| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 可以免费看污污视频的网站-日韩欧美不卡视频在线观看| 国产精品电影在线一区-亚洲国产大片一区二区官网| 亚洲视频一区二区三区免费-国产一级黄色大片在线| 91九色蝌蚪丝袜人妻-国产精品9999网站| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 久久夜色精品亚洲噜国产av-大香蕉伊人猫咪在线观看| av网址在线直接观看-黄色av全部在线观看| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 国产欧美日韩精品一区在线-久久精品视频免费获取地址| 欧洲精品一区二区三区中文字幕-91久久国产综合久久蜜月精品| 少妇人妻无码久久久久久-综合图片亚洲网友自拍| 久久精品亚洲国产av久-国产精品视频一区二区免费| 91大神国内精品免费网站-亚洲免费电影一区二区| 日韩二级视频在线观看-美女扒开奶罩露出奶子的视频网站| 91蜜桃传媒一二三区-日韩欧美国产一区呦呦| 亚洲国产日韩精品四区-dy888午夜福利精品国产97| 欧美精品啪啪人妻一区二区-嫩草人妻舔舔羞羞一区二区三区| 蜜臀av日日欢夜夜爽一区-av在线免费永久播放| 精彩亚洲一区二区三区-中文字幕中文字幕在线色站| 男女做爰猛烈啪啪吃奶在线观看-人妻连裤丝袜中文字幕| 日韩精品亚洲不卡一区二区-成人网在线视频精品一区二区三区|