欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

Why should we study nanoceramic bonded carbide? As we all know, WC-Co carbide consists of hard phase (WC) and bonding phase (ferrous metal). In harsh environments, the bonding phase is more susceptible to corrosion and oxidation than the hard phase, which limits its application in some fields. Therefore, reducing the content of the bonding phase is considered to solve this problem. In addition, metal Co is an expensive material and has a certain impact on human health. It is necessary to reduce the application of Co in carbide from the perspective of reducing costs and human health.

Nanoceramic bonded phase WC-based carbide refers to a type of carbide product that does not contain or contains a small amount of metal bonding agent (<0.5% by mass fraction). It has unparalleled excellent wear resistance, corrosion resistance, excellent polishing, and oxidation resistance compared to traditional carbide.

nanoceramic bonded phase WC-based carbide is a combination of ceramic hardness and carbide toughness, and products have been launched abroad. With its excellent wear and corrosion resistance, it can be used to make sandblasting nozzles, electronic packaging materials, heavy-duty sliding seal wear-resistant parts, etc.. with its excellent cutting performance, it can be used as tool and drill materials, especially for processing titanium/titanium alloys, which greatly improves work efficiency. and with its oxidation resistance and excellent polishing, it can be used as mold and decorative materials.

nanoceramic bonded carbide's micro structure

Characteristics of nanoceramic bonded carbide:

1Phase structure and carbon content of nanoceramic bonded phase carbide carbide are very sensitive to carbon content. For traditional carbide containing bonding phases, there is a certain range of carbon content to maintain a normal phase structure. If this range is exceeded, brittle n-phase or free carbon will appear. In contrast, the suitable carbon content of nanoceramic bonded phase WC-based carbide is not fluctuating like WC-Co alloy but is a fixed value.

2Composition design and properties of nanoceramic bonded carbide

Nanoceramic bonded carbide, which combine mechanical and wear resistance properties perfectly, are one of the most widely used ceramic-based materials in engineering. However, in most ceramic-based materials, the existence of metal bonding phases not only makes these composite materials have excellent flexural toughness but also affects certain properties, which limits their use. In addition, the low melting point of metal Co also greatly limits the application of WC-Co cutting tools in high-speed machining, which is prone to serious adhesive wear and oxidation wear. Moreover, the poor corrosion resistance, high cost, and toxicity of Co also limit the mechanical industry application of WC-Co carbide. Therefore, partially or completely replacing the Co bonding phase can expand the application of carbide. In recent years, ceramic bonding phases have attracted widespread attention in the scientific community as a new type of Co substitute.

 

The specific study using Nanoceramics as Binder Phase in Hardmetal Alloys

The Research Institute of Shandong University in China selected nanoscale Al2O3, ZrO2, and MgO as the binder phase for WC hardmetal alloys. The microstructure and mechanical properties of the hardmetal alloys were compared, and the toughening mechanism of the nanoceramic oxides was explored. The related paper, titled “Nano-ceramic replacing cobalt in cemented carbide as binder phase: Is it feasible?”, was published in the Journal of Alloys and Compounds.

Paper link:

https://linkinghub.elsevier.com/retrieve/pii/S0925838821043784

 

What is nanoceramic bonded carbide? 1

 

 

 

 

4Mechanism of Ceramic Binders Improving Toughness of carbide?Materials

What is nanoceramic bonded carbide? 2

fig.1 TEM micrographs of nanoceramic bonded carbide: (a) dislocations in WC-6Al2O3, (b) dislocations in WC-6ZrO2, (c) dislocations in WC-6MgO, and (d) intragranular and intergranular microstructures of WC-6ZrO2.

After sintering, the WC grains retained their initial grain size, and the second phase significantly suppressed the grain growth of the WC matrix by limiting grain boundary migration. Dislocations were observed in all three nanoceramic bonded carbide materials, which enhanced the tolerance of the carbide. Additionally, it was found that some nanoscale ZrO2 grains were distributed along the WC grain boundaries, while more ZrO2 nanograins were distributed within the WC grains, forming so-called intragranular nanostructures. Compared with the ceramic binder phase at the WC grain boundaries, the ceramics inside the WC grains were smaller in size.

What is nanoceramic bonded carbide? 3

fig.2 The toughening mechanism of WC-6Al2O3

What is nanoceramic bonded carbide? 4

fig.3 The toughening mechanism of WC-6ZrO2

What is nanoceramic bonded carbide? 5

fig.4 The toughening mechanism of WC-6AMgO

During the high-temperature sintering and cooling process, residual tensile stresses are generated around the ceramic binder phase due to differences in thermal expansion coefficient, which is favorable for crack deflection when the crack reaches the stress field. When an external load is applied to the nano-ceramic binder material, the difference in elastic modulus causes a redistribution of microscopic stress, thereby increasing the material’s toughness. All three nanoceramic bonded carbide materials exhibit crack bridging, effectively reducing crack propagation energy. Non-branching cracks were also found in the carbide, greatly increasing the energy consumption of the main crack propagation and effectively slowing down crack propagation.

What is nanoceramic bonded carbide? 6

fig.5 XRD spectra of the polished surface and fractured surface of the WC-6ZrO2 specimen

During the fracture process of WC-ZrO2 carbide, when external stress is applied to the carbide, stress concentration occurs near the crack tip, promoting the transformation of t-ZrO2 to monoclinic m-ZrO2. This transformation significantly impedes the crack propagation by enhancing stress relaxation near the crack tip. In addition, the volume expansion caused by phase transformation compresses the surrounding matrix, which is conducive to crack closure. Furthermore, surface phase transformation can generate compressive stress, greatly increasing the toughness of the material.

??

In summary, compared with traditional WC-Co carbide, nanoceramic bonded carbide exhibit a better combination of fracture toughness and hardness. Compared with micro-ceramic bonded? carbide, the hardness and fracture toughness of nano-ceramic bonded phase carbide are simultaneously enhanced. This excellent hardness of nano-ceramic bonded phase carbide is crucial for high-speed machining applications and is expected to become a candidate material for high-speed machining tools.

?? ???

???? ???? ????. ?? ???? * ? ???? ????

91蜜桃传媒一二三区-日韩欧美国产一区呦呦| 91九色蝌蚪丝袜人妻-国产精品9999网站| 97香蕉久久国产在线观看-麻豆黄色广告免费看片| 日韩精品一区二区三区粉嫩av-欧美亚洲国产中文字幕| 日韩亚洲欧美综合在线-成人在线网站在线观看| 久久免费观看归女高潮特黄-黄色av一本二本在线观看| 日本韩国亚洲欧美三级-日本东京不卡网一区二区三区| 国产一区二区三区四区五区麻豆-欧美一级在线视频播放| 久久精品国产96精品-日韩人成理论午夜福利| 18禁真人在线无遮挡羞免费-中文字幕精品一区二区三区四区| 亚洲欧洲成视频免费观看-国产福利一区二区在线观看| 欧美亚洲另类久久久精品-国产精品一区二区亚洲推荐| 国产精品二区高清在线-91精品91久久久久久| 国产欧美日韩精品一区在线-久久精品视频免费获取地址| 色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 亚洲av专区在线观看国产-丰满人妻av一区二区三区| 精品国产综合一区二区三区-蜜臀一区二区三区刺激视频| 欧美日韩国产在线资源-超碰成人国产一区二区三区| 精品亚洲卡一卡2卡三卡乱码-一区三区二插女人高潮在线观看| 免费av一区在线观看-国产精品视频高潮流白浆视频免费| 丝袜高跟熟女视频国产-熟女少妇亚洲一区二区| 一级小黄片在线免费看-亚洲欧美午夜情伊人888| 两性污污视频网站在线观看-亚洲欧美日韩激情一区| 免费av一区在线观看-国产精品视频高潮流白浆视频免费| 久久特一级av黄色片-91社区视频免费观看| 亚洲黄片三级三级三级-国产成人一区二区在线视频| 午夜福利1区2区3区-午夜洗澡免费视频网站| 国产黄片在现免费观看-色老板最新在线播放一区二区三区| 国产欧美日韩中文字幕在线-国产伊人一区二区三区四区| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 欧美一区二区三区调教视频-三上悠亚国产精品一区二区三区| 三上悠亚免费观看在线-青青草原在线视频观看精品| 欧美亚洲另类久久久精品-国产精品一区二区亚洲推荐| 欧美精品一区二区不卡-精品国产一区二区三区香蕉网址| 国产成人高清精品免费5388-好妞色妞在线视频播放| 99久热精品免费观看四虎-亚洲天堂精品视频在线| 国产综合日韩激情在线-日韩精品人妻一专区二区三区| 亚洲视频一区二区三区免费-国产一级黄色大片在线| 日韩高清在线观看一区二区-美产av在线免费观看| 久久免费观看归女高潮特黄-黄色av一本二本在线观看| 99在线免费观看视频-丰满人妻一区二区三区视频53|