Cemented carbide is a significant type of cemented carbide, widely used in manufacturing cutting tools, wear-resistant parts, high-temperature alloy components, and other important applications. Factors such as extrusion forming processes, forming agents, sintering atmosphere, and magnetic properties all impact the performance and quality of WC+Co alloy. Studying the effects and mechanisms of these factors is crucial for optimizing the manufacturing process and enhancing the performance of cemented carbide. This article will explore the influence of sintering atmosphere and particle size on the quality of the extrusion forming process, providing theoretical and practical guidance for further understanding the manufacturing process and performance optimization of cemented carbide.

cemented carbide

Experimental Materials and Methods

Tungsten carbide (WC) powders were used as the raw material. Four different particle sizes of WC powder were selected: 4.0 μm, 2.2 μm, 1.1 μm, and 0.5 μm, which were labeled as WC1, WC2, WC3, and WC4, respectively. Metal cobalt (Co) powder was used as the binder phase, and paraffin was used as the forming agent. Four different WC-Co mixtures with varying particle sizes were prepared.

The mixtures were processed into green bodies with specific shapes and densities using extrusion forming equipment. The pressed green bodies were then placed in a sintering furnace and subjected to high-temperature sintering at 1400°C for 30 minutes, followed by cooling, to form cemented carbide bars.

The magnetic properties of the cemented carbide bars were tested using a magnetic performance tester, measuring parameters such as coercive force (Hc) and saturation magnetization (Bs), and the results were analyzed.

 

Experimental Results and Analysis

Table 1 presents the effects of different WC particle sizes on the coercive force (Hc) and saturation magnetization (Bs) of cemented carbide bars.
Table 1 presents the effects of different WC particle sizes on the coercive force (Hc) and saturation magnetization (Bs) of cemented carbide bars.

Effect of Particle Size on Coercive Force

As shown in Table 1, the coercive force of cemented carbide bars increases with decreasing WC particle size, while the saturation magnetization also increases. This indicates that cemented carbide bars made with fine and ultrafine WC particles exhibit poorer magnetic properties. Among the samples, the ultrafine WC (WC4) shows the highest coercive force of 4450 A/m, followed by medium-sized WC (WC3) with a coercive force of 3300 A/m. Coarse WC (WC2) and very coarse WC (WC1) have lower coercive forces, at 2350 A/m and 1200 A/m, respectively. The increase in coercive force with decreasing WC particle size is primarily due to the increase in internal defects and dislocations within smaller particles. These defects and dislocations create resistance to domain wall movement, making the magnetization process more difficult and requiring a larger external magnetic field to achieve saturation, thereby increasing the coercive force.

 

Effect of Particle Size on Material Magnetic Performance Stability

For fine and ultrafine WC particles, the larger grain boundary area facilitates grain boundary diffusion and reactions, which reduces the material’s magnetic properties. As the WC particle size decreases, the magnetic saturation of cemented carbide bars gradually increases. Specifically: coarse WC (WC1) exhibits the lowest magnetic saturation at only 1.25 T; medium-sized WC (WC2) has a magnetic saturation of 1.15 T; fine WC (WC3) and ultrafine WC (WC4) show higher magnetic saturations at 1.05 T and 0.93 T, respectively. This is likely because fine and ultrafine WC particles have higher chemical reactivity, promoting the diffusion and bonding of the Co binder, thereby improving the stability of the material’s magnetic performance.

Magnetic saturation is an indicator of the remaining proportion of magnetizable material and is closely related to magnetic properties such as coercive force and remanence. The impact of WC particle size on magnetic saturation can be attributed to the degree of solubility of the binder phase in the cemented carbide bars. Coarse and medium-sized WC particles, having larger specific surface areas, have more contact with the Co binder, which enhances the solubility of Co in the cemented carbide bars. This effectively improves the material’s magnetic performance stability, resulting in higher coercive force and better magnetic stability. Conversely, fine and ultrafine WC particles, with smaller specific surface areas, reduce the effectiveness of the Co binder, potentially affecting the material’s hardness and magnetic properties. Thus, selecting the appropriate particle size during the preparation of cemented carbide bars is crucial for achieving the best overall performance based on specific application needs.

 

Impact of Gamma Phase on Material Performance

For cemented carbide materials, the proportion of the gamma phase directly affects the material’s hardness and magnetic properties. Variations in carbon and oxygen content also influence the gamma phase proportion and must be considered during material preparation. Generally, higher carbon content leads to an increase in the gamma phase proportion, thereby enhancing the material’s hardness and magnetic performance. Therefore, different WC particle sizes may have varying carbon and oxygen contents, which also affects the gamma phase proportion and the overall performance of the material.

 

Discussion on Sintering Atmosphere

In the sintering process of cemented carbides, the choice and control of the atmosphere have a decisive impact on the final microstructure and magnetic properties of the material. The atmosphere not only affects the chemical reactions during sintering but also directly relates to the microstructure and final performance of the cemented carbide. The types of sintering atmospheres are as follows:

Oxidizing Atmosphere:? air.

Reducing Atmosphere: Contains components such as H? or CO: hydrogen atmosphere for cemented carbide sintering.

Inert or Neutral Atmosphere: Argon, helium, vacuum.

Carburizing Atmosphere: Contains high components that cause carburization of the sintered body, such as CO, methane, and hydrocarbon gases.

Nitrogen-Based Atmosphere: High nitrogen content sintering atmosphere: 10% H? in N?.

We mainly selected vacuum, argon, and hydrogen atmospheres for discussion. The variations in coercive force and magnetic saturation of cemented carbides sintered in argon, vacuum, and hydrogen atmospheres differ depending on the atmosphere, as shown in Table 2.

Table 2: Effects of Different Sintering Atmospheres on Magnetic Properties of Cemented Carbide Bars
Table 2: Effects of Different Sintering Atmospheres on Magnetic Properties of Cemented Carbide Bars

From Table 2, it can be observed that under vacuum and argon atmospheres, the coercive force (Hc) of cemented carbide bar is higher compared to that in a hydrogen atmosphere. Conversely, the saturation magnetization (Bs) is lowest in a hydrogen atmosphere compared to vacuum and argon atmospheres.

Under vacuum and argon atmospheres, the effective control of oxygen partial pressure and the exclusion of volatile elements result in fewer pores and inclusions, clearer grain boundaries, and better grain growth, thereby enhancing the magnetic properties of the material. In contrast, in a hydrogen atmosphere, the reducing nature of hydrogen may reduce some elements in the cemented carbide, leading to the presence of uncertain phase components, poor grain growth, and subsequently affecting the material’s magnetic properties.

For coercive force (Hc), it is largely dependent on the material’s microstructure and magnetic anisotropy. Under vacuum and argon atmospheres, effective control of oxygen partial pressure and exclusion of volatile elements reduce magnetic anisotropy in the cemented carbide, which improves coercive force. However, in a hydrogen atmosphere, hydrogen’s reducing effect can lead to the reduction of some elements in the cemented carbide, resulting in grain defects and inclusions that directly affect magnetic anisotropy and reduce coercive force.

Regarding saturation magnetization (Bs), the relative magnetic saturation value in cemented carbide is influenced by factors affecting carbon content in the alloy. In vacuum or argon atmospheres, effective control of oxygen content reduces carbon loss. Although the pressed green body contains oxygen, which can be reduced by free carbon and carbon in WC (MeO + C = Me + CO), the oxygen content in these atmospheres is relatively low. In a hydrogen atmosphere, decarburization reactions (WC + 2H? → CH? + C) begin at around 100°C. Throughout the preparation process, the material is exposed to a decarburizing atmosphere, leading to a lower relative magnetic saturation value.

How Do Sintering Atmosphere and Particle Size Affect the Extrusion Forming Quality of Cemented Carbide Bars? 2

結(jié)論

This experiment investigated the effects of different particle sizes and sintering atmospheres on the magnetic properties of cemented carbide bars. By comparing the magnetic properties of cemented carbide under different WC particle sizes (coarse, medium, fine, and ultrafine) and sintering atmospheres (vacuum, argon, and hydrogen), it was found that both particle size and atmosphere have a significant impact on the magnetic performance of the material.

From the perspective of particle size, as the WC particle size decreases, the coercive force of the cemented carbide bars increases, while magnetic saturation also increases. This indicates that particle size has a substantial effect on the magnetic properties of cemented carbide. Fine and ultrafine WC particles, due to their higher chemical reactivity and good sintering performance, can promote the diffusion and bonding of the Co binder, thus enhancing the stability of the material’s magnetic performance. However, smaller particle sizes may lead to increased porosity and inclusions, affecting the material’s hardness and magnetic performance. Therefore, the choice of particle size should be tailored to the specific application needs when preparing cemented carbide.

Regarding the atmosphere, cemented carbide bars sintered under vacuum and argon atmospheres exhibited higher coercive force and better magnetic stability. This is because these atmospheres effectively control the oxygen content and volatile elements, reducing porosity and inclusions, and promoting clearer grain boundaries and grain growth. In contrast, cemented carbide bars sintered in a hydrogen atmosphere showed significantly lower magnetic saturation. This is likely due to the decarburizing effect of hydrogen. Therefore, selecting the appropriate sintering atmosphere is crucial for obtaining cemented carbide bars with excellent magnetic properties. Further improvements in cemented carbide performance can be achieved by optimizing sintering process parameters and adding suppressants.

9月 4, 2024

Meilleur matériaux TOP

コメントを殘す

メールアドレスが公開されることはありません。 が付いている欄は必須項目です

留学生美女被大黑屌猛戳| 美国大鸡巴操逼视频| 国产一区二区三区在线观| 欧美亚洲另类天天综合网| 粉嫩小穴被大鸡巴操视频在线观看| 日本免费无码一区二区到五区| 强奸啪啪啪好大欧美| 美女被操的流水AV| 丁香婷婷色婷婷粗大| 一区二区国产精品免费视频| 国产免费好大好硬| 亚洲一区二区三区大胆视频| 青青河边草直播免费观看| 欧美日韩久久久一区二区三区| 性色av一区二区三区天美传媒四| 被下药强奷到舒服的视频| 少妇勾搭外卖员在线观看| 日韩人妻精品一区二区三区| 欧美老熟妇又粗又大| 女人被男人躁爽色欲国产| 中文字幕欧美中日韩精品| 操你的骚逼粉嫩AV| 成人黄色网破处在线播放| 久久精品欧美日韩精品不卡| 精品人妻少妇一区二区三区不卡| 粗大长内射女人视频| 女人被大鸡吧操逼| 日国产精品1卡二卡三卡| 精品麻豆国产免费一区二区三区| 日韩在线视频不卡一区二区三区| 那种视频在线观看你懂的| 精品无码国产一区二区三区麻豆| 国产综合精品一区二区青青| 亚洲国产AV精品一区二区色欲| 骚逼嫩鸡巴喷水视频| 我最爱操女人的骚逼| 成人黄色精品久久app| 大鸡扒干美女BB直流水| 午夜场射精嗯嗯啊啊视频| 公交车上被后入搞逼漫画| 99爱这里只有精品|