In recent years, the production technology of ultra-fine grain cemented carbide has developed rapidly, especially in the key technology of preparing ultra-fine grain WC powder, where the competition is very fierce. Many promising methods have emerged, some of which have reached the level of practical application. However, there are few reports in domestic literature, especially on basic theories or regularity research. In the process of developing the preparation technology of ultra-fine grain WC powder, this paper deeply investigates the influence of the particle size of carbon black powder on the carbon content of WC powder under different carbonization temperatures when using ultra-fine (0.35 μm) tungsten powder.

 

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 2

Experimental Content and Method

Test Materials of WC powder

(1) Ultra-fine tungsten powder: The ultra-fine tungsten powder is prepared by the ultrasonic spray pyrolysis method from ultra-fine WO? powder, which is generally amorphous with an average particle size of 25~30 nm. It is reduced by hydrogen at a medium temperature (750~780℃) to obtain tungsten powder with an average particle size of ≤0.35μm (BET particle size).

(2) Carbon black powder: Carbon black powder is produced by two methods: one is by cracking ethane and propane (at 850℃) and then subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.1 and 0.3 μm, respectively; the other is from activated carbon powder with an original particle size of 100~200μm, which is subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.8 and 4.5 μm, respectively.

Experimental Method

Using ultra-fine tungsten powder with the same particle size (0.35 μm) and four different particle sizes (0.1, 0.3, 0.8, 4.5 μm) of carbon black powder, the carbon is blended according to the reaction formula W+C=WC (with an additional loss of 0.1%). The mixture is ball milled for 1.5 hours in a conventional ball mill with a ball-to-material ratio of 1:1. The heat-resistant stainless steel boat containing the mixed material is placed in a stainless steel tube furnace and carbonized under a hydrogen atmosphere. The holding time is 40 minutes for all. In the temperature range of 830~1300℃, the carbonized material is taken out at different temperatures, cooled, and then removed from the furnace. Subsequently, XRD phase analysis and chemical analysis are conducted to determine the total carbon and free carbon, and the amount of combined carbon in WC is calculated. Finally, the quantitative relationship between the particle size of carbon black powder and the phase composition and combined carbon content of WC powder under different carbonization temperatures can be plotted.

 

Test Results and Discussion

Figure 1 shows the effect of carbon black powder with different particle sizes carbonized at different temperatures on the combined carbon content of WC powder. Curve 1 in Figure 1 represents the relationship between carbonization temperature and the combined carbon content of WC powder when using ultra-fine carbon black powder with a particle size of 0.1 μm. As can be seen from Figure 1, when using 0.1 μm ultra-fine carbon black, the combined carbon content of WC powder can reach 5.8% (by mass), which is equivalent to 95% of the theoretical content, at a very low carbonization temperature (850℃). When the temperature is greater than 950℃, the carbon content of WC powder can reach the theoretical content. This result indicates that the carbonization reaction can be completed at a low temperature when using ultra-fine tungsten powder in conjunction with ultra-fine carbon black powder. This phenomenon suggests that the ultra-fine W powder particles are carbonized before they undergo significant aggregation and growth.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 3
At this temperature, as the particle size of the carbon black used increases, the combined carbon content in WC powder rapidly decreases. For example, as shown in Curve 2 of Figure 1, when using 0.3 μm carbon black at 950℃ with the same holding time of 40 minutes, the combined carbon content of WC powder only reaches 5.2% (by mass). XRD analysis indicates that there is still significant W?C in the WC powder, as shown in Figure 2. The free carbon phase was not detected due to its low content. The combined carbon content in WC powder can only reach the theoretical value when the temperature is increased to 1060℃. Its complete carbonization temperature is about 130℃ higher than that of the 0.1 μm carbon black.

カーボンブラック粒子サイズがWC粉末の炭素含有量に與える影響4

When using 0.8 μm carbon black, as shown in Curve 3 of Figure 1, at 950℃ with a holding time of 40 minutes, the combined carbon content of WC is only 3.18% (by mass). XRD analysis indicates that in addition to the obvious W?C phase, there is also significant free carbon present in the WC powder, as shown in Figure 3. The combined carbon content in WC powder can only reach the theoretical value when the carbonization temperature is increased to 1230℃. The temperature required for complete carbonization has increased significantly.
The reason for this phenomenon is that when the carbon content ratio is constant, the finer the carbon black particle size, the easier it is to mix uniformly with W powder particles, increasing the contact area between them. Undoubtedly, fine-grained carbon black will accelerate the carbonization rate. Moreover, the finer the carbon black particle size, the more its specific surface area and the number of active carbon atoms on the surface increase dramatically. Thus, the carbonization reaction rate between carbon and tungsten accelerates, and the complete carbonization temperature decreases with the decrease of carbon black particle size.

WC powder

Conclusions

(1) When the particle size of ultra-fine W powder is the same (≤0.35μm), the combined carbon content in WC powder decreases significantly with the increase of the carbon black particle size at a certain temperature.
(2) When the particle size of carbon black is constant, the content of combined carbon increases with the rise of carbonization temperature.

コメントを殘す

メールアドレスが公開されることはありません。 が付いている欄は必須項目です

小穴抽插流水视频| 无码中文字幕免费一区二区三区| 激情久久久久久久久久久| 久久婷婷综合五月一区二区| 爆乳喷奶水无码正在播放| 国产免费无码一区二区视频无码| 国产精品免费久久久久久| 精品一区二区三区乱码中文字幕| 欧美猛男一区二区三区快播| 大香蕉操逼小视频| 久久久国产系列丝袜熟女| 干女人逼逼的大几把| 丁香婷婷色婷婷粗大| 美女穿黑丝被大鸡巴猛操| 亚洲欧美日韩另类| aaa啊啊啊黄片| 欧美 日韩 激情 在线| av中文字幕一区二区精品久久| 乱伦美女小骚货视频| 大鸡巴操逼 公司| 高颜值美女视频在线观看| 久久久精品国产乱码内射| 多男用舌头伺候一女| 日本乱人伦中文在线播放| 亚洲一区亚洲二区在线观看| 大鸡巴操逼视频免费| 日韩精品无码一区二区三区不卡| 欧美人与性动交b欧美精品| 夜色成人免费观看| 中文字幕你懂的av一区二区| 手机成人三级a在线观看| 中文字幕欧美人妻在线| 影音先锋亚洲中文综合网| 999久久久国产大美腿| 我要操死你逼视频| 男人的下面进女人的下面在线观看| 美性中文网中文字幕91| 亚洲精品自拍偷拍第一页| 中文字幕 av一区二区| 欧美va精品亚洲va精品| 粗大长内射女人视频|