欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

In recent years, the production technology of ultra-fine grain cemented carbide has developed rapidly, especially in the key technology of preparing ultra-fine grain WC powder, where the competition is very fierce. Many promising methods have emerged, some of which have reached the level of practical application. However, there are few reports in domestic literature, especially on basic theories or regularity research. In the process of developing the preparation technology of ultra-fine grain WC powder, this paper deeply investigates the influence of the particle size of carbon black powder on the carbon content of WC powder under different carbonization temperatures when using ultra-fine (0.35 μm) tungsten powder.

 

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 2

Experimental Content and Method

Test Materials of WC powder

(1) Ultra-fine tungsten powder: The ultra-fine tungsten powder is prepared by the ultrasonic spray pyrolysis method from ultra-fine WO? powder, which is generally amorphous with an average particle size of 25~30 nm. It is reduced by hydrogen at a medium temperature (750~780℃) to obtain tungsten powder with an average particle size of ≤0.35μm (BET particle size).

(2) Carbon black powder: Carbon black powder is produced by two methods: one is by cracking ethane and propane (at 850℃) and then subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.1 and 0.3 μm, respectively; the other is from activated carbon powder with an original particle size of 100~200μm, which is subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.8 and 4.5 μm, respectively.

Experimental Method

Using ultra-fine tungsten powder with the same particle size (0.35 μm) and four different particle sizes (0.1, 0.3, 0.8, 4.5 μm) of carbon black powder, the carbon is blended according to the reaction formula W+C=WC (with an additional loss of 0.1%). The mixture is ball milled for 1.5 hours in a conventional ball mill with a ball-to-material ratio of 1:1. The heat-resistant stainless steel boat containing the mixed material is placed in a stainless steel tube furnace and carbonized under a hydrogen atmosphere. The holding time is 40 minutes for all. In the temperature range of 830~1300℃, the carbonized material is taken out at different temperatures, cooled, and then removed from the furnace. Subsequently, XRD phase analysis and chemical analysis are conducted to determine the total carbon and free carbon, and the amount of combined carbon in WC is calculated. Finally, the quantitative relationship between the particle size of carbon black powder and the phase composition and combined carbon content of WC powder under different carbonization temperatures can be plotted.

 

Test Results and Discussion

Figure 1 shows the effect of carbon black powder with different particle sizes carbonized at different temperatures on the combined carbon content of WC powder. Curve 1 in Figure 1 represents the relationship between carbonization temperature and the combined carbon content of WC powder when using ultra-fine carbon black powder with a particle size of 0.1 μm. As can be seen from Figure 1, when using 0.1 μm ultra-fine carbon black, the combined carbon content of WC powder can reach 5.8% (by mass), which is equivalent to 95% of the theoretical content, at a very low carbonization temperature (850℃). When the temperature is greater than 950℃, the carbon content of WC powder can reach the theoretical content. This result indicates that the carbonization reaction can be completed at a low temperature when using ultra-fine tungsten powder in conjunction with ultra-fine carbon black powder. This phenomenon suggests that the ultra-fine W powder particles are carbonized before they undergo significant aggregation and growth.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 3
At this temperature, as the particle size of the carbon black used increases, the combined carbon content in WC powder rapidly decreases. For example, as shown in Curve 2 of Figure 1, when using 0.3 μm carbon black at 950℃ with the same holding time of 40 minutes, the combined carbon content of WC powder only reaches 5.2% (by mass). XRD analysis indicates that there is still significant W?C in the WC powder, as shown in Figure 2. The free carbon phase was not detected due to its low content. The combined carbon content in WC powder can only reach the theoretical value when the temperature is increased to 1060℃. Its complete carbonization temperature is about 130℃ higher than that of the 0.1 μm carbon black.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 4

When using 0.8 μm carbon black, as shown in Curve 3 of Figure 1, at 950℃ with a holding time of 40 minutes, the combined carbon content of WC is only 3.18% (by mass). XRD analysis indicates that in addition to the obvious W?C phase, there is also significant free carbon present in the WC powder, as shown in Figure 3. The combined carbon content in WC powder can only reach the theoretical value when the carbonization temperature is increased to 1230℃. The temperature required for complete carbonization has increased significantly.
The reason for this phenomenon is that when the carbon content ratio is constant, the finer the carbon black particle size, the easier it is to mix uniformly with W powder particles, increasing the contact area between them. Undoubtedly, fine-grained carbon black will accelerate the carbonization rate. Moreover, the finer the carbon black particle size, the more its specific surface area and the number of active carbon atoms on the surface increase dramatically. Thus, the carbonization reaction rate between carbon and tungsten accelerates, and the complete carbonization temperature decreases with the decrease of carbon black particle size.

WC powder

Conclusions

(1) When the particle size of ultra-fine W powder is the same (≤0.35μm), the combined carbon content in WC powder decreases significantly with the increase of the carbon black particle size at a certain temperature.
(2) When the particle size of carbon black is constant, the content of combined carbon increases with the rise of carbonization temperature.

Lascia un commento

Il tuo indirizzo email non sarà pubblicato. I campi obbligatori sono contrassegnati *

色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 黄色美女网站大全中文字幕-欧美韩国日本一区二区| 国产一区二区无套内射-国内精品久久久久久久齐pp| 亚洲黄片三级三级三级-国产成人一区二区在线视频| 欧美日韩国产在线资源-超碰成人国产一区二区三区| 五月婷婷免费观看视频-男人操女人下面视频在线免费看| 熟女熟妇伦51788-国产av在线播放一区二区三区| 可以免费看污污视频的网站-日韩欧美不卡视频在线观看| 欧美看片一区二区三区-人妻无卡精品视频在线| 欧美日本亚一级二级三区久久精品-日韩欧美一区二区久久婷婷| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 亚洲区欧美区在线视频-亚洲碰碰人人AV熟女天堂| 欧美亚洲另类久久久精品-国产精品一区二区亚洲推荐| 午夜福利1区2区3区-午夜洗澡免费视频网站| 人妻日韩精品中文字幕图片-麻豆极度性感诱人在线露脸| 精彩亚洲一区二区三区-中文字幕中文字幕在线色站| 欧美视频在线观看国产专区-亚洲91精品在线观看| 美女把腿张开给帅哥桶-无码无套少妇18p在线直播| 久久精品国产96精品-日韩人成理论午夜福利| 久久夜色精品亚洲噜国产av-大香蕉伊人猫咪在线观看| 日韩毛片在线免费人视频-超碰中文字幕av在线| 天天干天天日天天射天天舔-精品香蕉视频官网在线观看| 国产免费高清av在线播放-成年人在线播放中文字幕| 在线成色中文综合网站-国产二区精品视频在线观看| 亚洲女人黄色录像一区-日韩av电影在线免费看| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 欧美伦乱淫老妇女激情吧-亚洲女邻居精品二区久久| 九九热这里只有精品九九-欧美日韩人妻精品一二三| 欧美日韩国产综合四区-爆操极品尤物熟妇14p| 精品亚洲卡一卡2卡三卡乱码-一区三区二插女人高潮在线观看| 99精品只有久久精品免费-蜜臀一区二区三区精品久久久| 九九热这里只有精品九九-欧美日韩人妻精品一二三| 午夜精品午夜福利在线-内射无套内射国产精品视频| 亚洲av成人一区国产精品网-国产偷_久久一级精品a免费| 一区二区三区国产高清mm-美女张开腿让帅哥桶爽| 日韩亚洲一区二区三区av-欧美综合在线观看一区二区三区| 午夜福利卫生纸福利院-一区二区三区久久亚洲| 久久亚州天堂一区二区-色噜噜色哟哟一区二区三区| 三上悠亚免费观看在线-青青草原在线视频观看精品| 欧美三级韩国三级日本三斤-日本不卡一区不卡二区|