The research and development of crystal plane in cemented carbides is one of the hotspots in the field of cemented carbides both domestically and internationally. The microstructure of the alloy determines its mechanical properties; in WC-Co cemented carbides, the grain size and distribution of the WC phase, as well as the substructure within the grains, are important factors affecting the material’s mechanical properties [10-13]. WC grains have a close-packed hexagonal structure (crystal system P-6m2, a=0.2906nm, c=0.2837nm)24, and the habit planes of WC grains are two basal planes and three prismatic planes. WC grains are prismatic in three-dimensional space, with the basal plane being parallel to the (0001) crystal plane and the prism plane being parallel to the (1-100) crystal plane 5. On the basis of this basic shape, some of the edges and corners are replaced by new crystal planes?6-21. Given that cemented carbides with specific orientations can produce excellent mechanical properties to meet special application requirements, we believe that it is necessary to conduct in-depth research.

This paper takes WC-12Co cemented carbide as the research object. Firstly, nano WC-Co composite powders were prepared by in-situ reduction carbonization reaction at different temperatures, and the composite powders were rapidly densified by discharge plasma sintering technology. The sintered blocks were systematically studied to analyze the effect of the in-situ reduction carbonization reaction temperature on the distribution characteristics of special crystal planes.

Experiment

The raw materials used in the experiment were carbon black, blue tungsten (purity 99.5wt.%, average particle size 50μm) and cobalt oxide (purity 98.5wt.%, average particle size 35μm). Carbon black, blue tungsten, and cobalt oxide were weighed according to the proportion for generating WC-12Co powder, and high-energy ball milling was carried out in a hard alloy ball mill jar with ethanol as the ball milling medium. The mixed powders were subjected to in-situ reduction carbonization reaction at 850°C, 900°C, and 1000°C in a vacuum environment, with a holding time of 1 hour. 2wt% of grain growth inhibitor was added to the composite powders prepared by in-situ reaction, and discharge plasma sintering densification was carried out. The sintering temperature was 1080°C, the holding time was 5 minutes, and the sintering pressure was 60MPa.

Materiale phase analysis was carried out on a Rigaku D/max-3c X-ray diffractometer with an acceleration voltage of 35kV and a current of 30mA, and a scanning rate of 2°/min. The micro-morphology of the powder was observed on a FEI-NovaNano SEM field emission scanning electron microscope.

Results and of Crystal Plane Distribution

Figure 1 shows the thermogravimetric (TG-DSC) curves of the nano WC-Co composite powder synthesized by in-situ reaction when heated to 1000°C at a heating rate of 10°C/min under Ar gas protection. From the change in the TG curve, it can be seen that as the temperature increases, the mass of the in-situ synthesized WC-Co composite powder decreases. When the temperature reaches 1000°C, the reaction ends, and the powder weight loss reaches nearly 6%. Throughout the heating process, the mass loss of the composite powder is divided into two stages: the first stage is from room temperature to 190°C, where there is a significant decrease in powder mass due to the ease of gas adsorption by nanoscale powders, and the gas desorbs and releases during the heating process, causing powder weight loss; the second stage is from 628°C to 1000°C, where the weight loss rate decreases from high to low. This is because the composite powder did not fully react during the low-temperature in-situ reduction carbonization reaction, and a secondary reaction occurred during the heating process, resulting in rapid weight loss of the powder.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 2

Figure 2 shows the nanoscale WC-Co composite powder prepared by in-situ reduction carbonization reaction at 850°C. The powder particle size is mainly distributed between 30~120nm, with an average particle size of ~83.4nm. The particles have a good sphericity, and spherical or quasi-spherical powders exhibit good dispersibility and flowability, which can effectively avoid hard agglomeration of the powder. This is beneficial for the uniform dispersion of the powder in the sintering mold, thereby ensuring the uniformity and density of the sintered bulk structure. The composite powder prepared by the in-situ reduction carbonization reaction is subjected to rapid sintering densification in an SPS system to obtain nearly fully dense WC-Co cemented carbide blocks. XRD tests are conducted on the alloy specimens in the direction perpendicular to the sintering pressure and in the direction parallel to the sintering pressure. The relative integral intensities (i.e., integral area) of the diffraction peaks for each crystal plane in the VD (vertical to the sintering pressure) and PD (parallel to the sintering pressure) planes of the specimens are obtained through fitting calculations and compared with the relative intensities (integral area) of the diffraction peaks for each crystal plane in the PDF card (which represents the diffraction peak intensity distribution characteristics of traditional sintered cemented carbides), as shown in Table 1. The results indicate that the sintered WC-Co cemented carbide block specimens exhibit a significant characteristic of high anisotropic distribution for specific crystal planes.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 3

Figure 3 shows the XRD patterns of the VD (vertical to the sintering pressure) and PD (parallel to the sintering pressure) planes of the specimens obtained by SPS sintering of the nanoscale WC-Co composite powder prepared by in-situ reaction at 850°C. From the figure, it can be observed that on the PD plane, the intensity of the (0001) plane peak is lower, while the intensity of the (10-10) plane peak is relatively higher. By fitting and calculating the integral area of each diffraction peak, the relative integral area of each crystal plane and the proportion of each crystal plane’s integral area in the total integral area are obtained, as shown in Figures 5 and 6.

 crystal plane distribution
crystal plane distribution

From Figure 5, it can be seen that on the PD plane, the integral area of the (0001) plane accounts for only 10.72% of the total integral area, which is a decrease of 3.3% from the 14.02% in the PDF card (as shown in Figure 4). The proportion of the (10-10) plane reaches 35.73%, which is higher than the 31.87% in the PDF card, and the proportion of the (10-11) plane decreases to 21.76% compared to the 28.11% in the PDF card. Compared to conventional cemented carbide samples, in the PD direction of the composite powder sintered block prepared by in-situ reaction at 850°C, the distribution proportion of the main characteristic planes (0001) and (10-11) decreases, while the distribution proportion of (10-10) increases.

 

Discussion

On the VD direction of the sample, as shown in Figure 6, the proportion of the (0001) crystal plane has significantly increased to 40%, compared to the 14.02% in the PDF card, while the proportion of the (10-10) crystal plane has decreased to 11.68%, a reduction of 20.19% from the 31.87% in the PDF card. From the above analysis, it can be understood that in the sintered block of composite powder prepared by in-situ reaction at 850°C, there is an orientation distribution of characteristic crystal planes. In the direction perpendicular to the pressure, WC grains rotate, causing the (0001) plane to become perpendicular to the pressure direction, thereby reducing the interfacial energy between WC grains. The sintered block of low-temperature in-situ reaction synthesis powder exhibits an orientation distribution characteristic of WC grain characteristic crystal planes, which is believed to be due to the formation of WC grains through secondary reactions during sintering, with atoms preferentially aligning along the (0001) plane and the rotation of WC grains under sintering pressure causing the (0001) plane to tend towards being perpendicular to the pressure direction.

When the temperature is raised to 900°C for in-situ reaction, the prepared composite powder is mainly WC with only a small amount of carbon-deficient phase. When the temperature is raised to 1000°C for in-situ reaction, pure WC-Co composite powder can be obtained. Since the crystal plane distribution of the grains in the powder is isotropic, the crystal plane distribution of WC grains does not change during the subsequent sintering densification process at 900°C and 1000°C, and they still exhibit a randomly distributed isotropic characteristic.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 4

Conclusione

1) The nanoscale WC-Co composite powder prepared by low-temperature in-situ reduction carbonization reaction at 850°C can be sintered into cemented carbide block materials with a highly oriented distribution characteristic of WC grain crystal planes using SPS. The sintered blocks of in-situ reaction powder at 900°C and 1000°C maintain an isotropic distribution of WC grain characteristic crystal planes.

2) In the WC-Co cemented carbide with highly oriented characteristic crystal planes, the basal plane (0001) occupies the largest area fraction in the direction perpendicular to the sintering pressure, reaching 40.0%; the prism plane (10-10) occupies the largest area fraction in the direction parallel to the pressure, reaching 35.7%.

3) The phase purity of the composite powder generated by the in-situ reaction plays an important role in the crystal plane orientation of the sintered block. When the main phase of the composite powder is WC, the crystal plane distribution of the sintered block does not exhibit oriented characteristics. However, when the main phase of the composite powder is the carbon-deficient phase, the crystal plane of the sintered block presents an oriented distribution characteristic.

Lascia un commento

Il tuo indirizzo email non sarà pubblicato. I campi obbligatori sono contrassegnati *

美女把腿张开给帅哥桶-无码无套少妇18p在线直播| 久久影视av一区二区-人妻激情乱偷一区二区三区| 97一区二区三区在线-欧美护士性极品hd4k| 男人的天堂久久精品激情-最新亚洲精品a国产播放| 日韩精品一区二区三区十八-日韩人妻少妇一区二区三区| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 亚洲黄片三级三级三级-国产成人一区二区在线视频| 欧美三级韩国三级日本三斤-日本不卡一区不卡二区| 91蜜桃传媒一二三区-日韩欧美国产一区呦呦| 成人av一区二区蜜桃-亚洲色图激情人妻欧美| 亚洲日本一区二区三区黄色电形-中文字幕乱码免费熟女| 欧美字幕一区二区三区-好吊妞欧美一区二区在线观看| 黑丝av少妇精品久久久久久久-中文字幕久久久人妻无码| 欧美成人精品巨臀大屁股-亚洲综合欧美日韩一区| 熟女少妇免费一区二区-麻豆一区二区三区免费在线观看| 国产精品熟女视频一区二区-国产日韩精品欧美一区喷水| 白嫩美女娇喘呻吟高潮-久久一区二区三区日产精品| 午夜福利卫生纸福利院-一区二区三区久久亚洲| 免费午夜福利在线观看-黄色日本黄色日本韩国黄色| 狠狠狠狠爱精品一二三四区-l舌熟女av国产精品| 日韩中文字幕v亚洲中文字幕-日韩亚洲av免费在线观看| 熟女熟妇伦51788-国产av在线播放一区二区三区| 国产在线一区二区三区欧美-久久偷拍精品视频久久| 乱入一二三免费在线观看-久久精品亚洲精品国产色婷婷| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 午夜日韩精品在线视频-亚洲网老鸭窝男人的天堂| 五月婷婷六月在线观看视频-亚洲黑寡妇黄色一级片| 亚洲黄片三级三级三级-国产成人一区二区在线视频| 国产一区二区无套内射-国内精品久久久久久久齐pp| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 国产在线不卡高清一区-日本一区二区三区四区无卡| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 国模自慰一区二区三区-日韩一级黄色片天天看| 午夜福利卫生纸福利院-一区二区三区久久亚洲| 99精品只有久久精品免费-蜜臀一区二区三区精品久久久| 成人免费资源在线观看-欧美国产日韩高清在线综合| 99在线观看精品视频免费-国产极品一区二区三区四区| 欧美日韩亚洲1区2区-黄污视频在线观看不卡| 交换朋友的妻子中文字幕-日本美女8x8x8x8| 日本欧美在线视频观看-国产一区二区三区无码下载快播| 成人av一区二区蜜桃-亚洲色图激情人妻欧美|