In recent years, the production technology of ultra-fine grain cemented carbide has developed rapidly, especially in the key technology of preparing ultra-fine grain WC powder, where the competition is very fierce. Many promising methods have emerged, some of which have reached the level of practical application. However, there are few reports in domestic literature, especially on basic theories or regularity research. In the process of developing the preparation technology of ultra-fine grain WC powder, this paper deeply investigates the influence of the particle size of carbon black powder on the carbon content of WC powder under different carbonization temperatures when using ultra-fine (0.35 μm) tungsten powder.

 

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 2

Experimental Content and Method

Test Materials of WC powder

(1) Ultra-fine tungsten powder: The ultra-fine tungsten powder is prepared by the ultrasonic spray pyrolysis method from ultra-fine WO? powder, which is generally amorphous with an average particle size of 25~30 nm. It is reduced by hydrogen at a medium temperature (750~780℃) to obtain tungsten powder with an average particle size of ≤0.35μm (BET particle size).

(2) Carbon black powder: Carbon black powder is produced by two methods: one is by cracking ethane and propane (at 850℃) and then subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.1 and 0.3 μm, respectively; the other is from activated carbon powder with an original particle size of 100~200μm, which is subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.8 and 4.5 μm, respectively.

Experimental Method

Using ultra-fine tungsten powder with the same particle size (0.35 μm) and four different particle sizes (0.1, 0.3, 0.8, 4.5 μm) of carbon black powder, the carbon is blended according to the reaction formula W+C=WC (with an additional loss of 0.1%). The mixture is ball milled for 1.5 hours in a conventional ball mill with a ball-to-material ratio of 1:1. The heat-resistant stainless steel boat containing the mixed material is placed in a stainless steel tube furnace and carbonized under a hydrogen atmosphere. The holding time is 40 minutes for all. In the temperature range of 830~1300℃, the carbonized material is taken out at different temperatures, cooled, and then removed from the furnace. Subsequently, XRD phase analysis and chemical analysis are conducted to determine the total carbon and free carbon, and the amount of combined carbon in WC is calculated. Finally, the quantitative relationship between the particle size of carbon black powder and the phase composition and combined carbon content of WC powder under different carbonization temperatures can be plotted.

 

Test Results and Discussion

Figure 1 shows the effect of carbon black powder with different particle sizes carbonized at different temperatures on the combined carbon content of WC powder. Curve 1 in Figure 1 represents the relationship between carbonization temperature and the combined carbon content of WC powder when using ultra-fine carbon black powder with a particle size of 0.1 μm. As can be seen from Figure 1, when using 0.1 μm ultra-fine carbon black, the combined carbon content of WC powder can reach 5.8% (by mass), which is equivalent to 95% of the theoretical content, at a very low carbonization temperature (850℃). When the temperature is greater than 950℃, the carbon content of WC powder can reach the theoretical content. This result indicates that the carbonization reaction can be completed at a low temperature when using ultra-fine tungsten powder in conjunction with ultra-fine carbon black powder. This phenomenon suggests that the ultra-fine W powder particles are carbonized before they undergo significant aggregation and growth.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 3
At this temperature, as the particle size of the carbon black used increases, the combined carbon content in WC powder rapidly decreases. For example, as shown in Curve 2 of Figure 1, when using 0.3 μm carbon black at 950℃ with the same holding time of 40 minutes, the combined carbon content of WC powder only reaches 5.2% (by mass). XRD analysis indicates that there is still significant W?C in the WC powder, as shown in Figure 2. The free carbon phase was not detected due to its low content. The combined carbon content in WC powder can only reach the theoretical value when the temperature is increased to 1060℃. Its complete carbonization temperature is about 130℃ higher than that of the 0.1 μm carbon black.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 4

When using 0.8 μm carbon black, as shown in Curve 3 of Figure 1, at 950℃ with a holding time of 40 minutes, the combined carbon content of WC is only 3.18% (by mass). XRD analysis indicates that in addition to the obvious W?C phase, there is also significant free carbon present in the WC powder, as shown in Figure 3. The combined carbon content in WC powder can only reach the theoretical value when the carbonization temperature is increased to 1230℃. The temperature required for complete carbonization has increased significantly.
The reason for this phenomenon is that when the carbon content ratio is constant, the finer the carbon black particle size, the easier it is to mix uniformly with W powder particles, increasing the contact area between them. Undoubtedly, fine-grained carbon black will accelerate the carbonization rate. Moreover, the finer the carbon black particle size, the more its specific surface area and the number of active carbon atoms on the surface increase dramatically. Thus, the carbonization reaction rate between carbon and tungsten accelerates, and the complete carbonization temperature decreases with the decrease of carbon black particle size.

WC powder

Conclusions

(1) When the particle size of ultra-fine W powder is the same (≤0.35μm), the combined carbon content in WC powder decreases significantly with the increase of the carbon black particle size at a certain temperature.
(2) When the particle size of carbon black is constant, the content of combined carbon increases with the rise of carbonization temperature.

Lascia un commento

Il tuo indirizzo email non sarà pubblicato. I campi obbligatori sono contrassegnati *

亚洲午夜久久久精品影院-性感美女在线观看网站国产| 日韩欧美国产综合久久-国产精品一起草在线观看| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 欧美成人精品巨臀大屁股-亚洲综合欧美日韩一区| 日韩中文字幕v亚洲中文字幕-日韩亚洲av免费在线观看| 国产免费一区二区三区不-日本少妇免费一区二区三区| 婷婷亚洲欧美综合丁香亚洲-超刺激国语对白在线视频| 亚洲综合av一区二区三区-高潮又爽又黄无遮挡激情视频| 国产精品中出久久久蜜臀-久久久中国精品视频久久久| 国产一区二区三区噜噜-精品久久亚洲一区二区欧美| 中文字幕精品一区二区日本99-青青国产成人久久91网| 美女把腿张开给帅哥桶-无码无套少妇18p在线直播| 亚洲精品在线观看一二三区-在线观看国产中文字幕视频| 国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 国产一级片久久免费看同-麻豆精品尤物一区二区青青| 国产在线一区二区三区欧美-久久偷拍精品视频久久| 91大神国内精品免费网站-亚洲免费电影一区二区| 97一区二区三区在线-欧美护士性极品hd4k| 人妻日韩精品中文字幕图片-麻豆极度性感诱人在线露脸| 久久夜色精品亚洲噜国产av-大香蕉伊人猫咪在线观看| 黄片免费观看视频下载-国产丝袜诱惑在线视频| 亚洲午夜久久久精品影院-性感美女在线观看网站国产| 国产一级片久久免费看同-麻豆精品尤物一区二区青青| 91精品国产影片一区二区三区-欧美精品久久久精品一区二区| 久久免费观看归女高潮特黄-黄色av一本二本在线观看| 黄色美女网站大全中文字幕-欧美韩国日本一区二区| 亚洲精品激情一区二区-久久成人国产欧美精品一区二区| 久色高清精品在线国产-国产精品视频一区三区四区| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 一区二区国产高清在线-日本高清无卡一区二区三区| 黄片黄片在线免费观看-激情综合网激情五月俺也去| 中文字幕精品一区二区日本99-青青国产成人久久91网| 久久精品亚洲无中文东京热-日本妹子内谢视频一区| 日韩精品一区二区三区十八-日韩人妻少妇一区二区三区| mm在线精品视频在线观看-欧美国产日韩在线一区二区三区| 99精品只有久久精品免费-蜜臀一区二区三区精品久久久| 91亚洲美女视频在线-熟妇人妻精品一区二区三区蜜臀| 白嫩美女娇喘呻吟高潮-久久一区二区三区日产精品| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 中文字幕日韩精品不卡一区二区-成人av在线观看一区二区| 一区二区国产高清在线-日本高清无卡一区二区三区|