Research status

For WC-Co carbide, the rapidly advancing Powder Bed Fusion (PBF) additive manufacturing (AM) technology has shown unique advantages in producing complex structures of metal parts made of carbide. However, when manufacturing WC-Co carbide with high melting points and high content of hard phases, issues such as difficult-to-eliminate cracks, pores, abnormal grain growth, oxidation decarburization, and brittleness often arise, leading to poor mechanical properties of the produced carbide. In recent years, there have been many reports on the use of Green Additive Manufacturing-Debinding and Sintering (GAM-DS) technology to fabricate WC-Co carbide, which have shown significant advantages in addressing issues such as cracking, abnormal grain growth, oxidation decarburization, and brittleness in PBF carbide. However, the process of preparing green bodies is prone to defects such as pores, interlayer cracks, uneven carbon distribution, and weak local bonding, resulting in problems such as porosity, uneven sintering shrinkage, and uneven microstructure in the sintered bodies. Compared with powder metallurgy, the prepared carbide have relatively low relative densities, and there is a significant gap in mechanical properties.

Brief introduction of research results

Recently, the State Key Laboratory of Powder Metallurgy at Central South University has employed Material Extrusion Additive Manufacturing (MEX) – Debinding and Sintering (DS) technology to successfully produce high-strength and tough WC-9Co cemented carbide with no pores, no cracks, and uniform shrinkage in all directions. Its relative density is approximately 99.7%, and its Vickers hardness, transverse fracture strength, and fracture toughness reach 1525±3HV30, 3492±45MPa, and 20.4±0.5 MPa·m1/2 respectively. The comprehensive mechanical properties are comparable to those of high-performance WC-Co carbide prepared by powder metallurgy processes. The relevant work, titled “Material extrusion additive manufacturing of WC-9Co cemented carbide,” was published in the top international journal “Additive Manufacturing.”

 

research chart

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 2

FIG. 1 Microstructure of MEX WC-9Co cemented carbide green

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 3

FIG. 2 Schematic diagram of stack pore formation of cemented carbide printing green billet: a. MEX stack pore formation; b. Increasing the overlap rate of microfilaments is conducive to reducing the stack porosity of green billet;

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 4

FIG. 3 Microstructure of MEX-DSWC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 5

Figure 4 Micro-CT analysis results of internal defects in MEX-DS WC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 6

Figure 5 Microstructure of WC-9Co cemented carbide: (a) MEX-DS; (b) Press forming – degreasing sintering

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 7

Figure 6 MEX-DS WC-Co carbide Co pool and Co rich zone

WC-Co carbide

Figure 7 Transverse fracture strength and fracture toughness of WC-(8-12)Co cemented carbide prepared by different processes

 

Riepilogo

Conclusion of the Paper

(1) By calculating the plasticity index of the printed feedstock with a powder loading of 54 Vol.%, the mechanism of green body printing defects was analyzed, and the green body MEX parameters were optimized. Using optimized parameters such as a printing temperature of 150°C, filament overlap rate of 30%, and printing layer thickness of 0.1mm, defect-free green bodies of WC-9Co cemented carbide with a relative density of 98.5% were prepared.

(2) Both excessively high or low temperatures during the debinding process using n-heptane can lead to debinding cracks. Rapid solvent evaporation during the drying process of debound bodies can also result in microcracks. By employing a two-step solvent debinding process, namely, n-heptane debinding at 30°C for 12 hours followed by kerosene debinding at 30°C for 1 hour, the solvent evaporation rate was reduced, resulting in high-quality debound bodies with no noticeable debinding defects and uniform distribution of binder.

(3) Defects in MEX green bodies can lead to the formation of Co-rich regions or pools, abnormal WC grains, residual pores, etc., in WC-Co carbide. These defects can be improved or eliminated during the sintering process through liquid phase flow and rearrangement of WC particles. By optimizing the MEX green body printing and solvent debinding processes to eliminate printing and debinding defects, it is possible to eliminate defects such as sintering pores, cracks, Co pools, abnormal grain growth, etc., in WC-Co carbide, resulting in near-full-density WC-9Co carbide.

(4) By employing MEX green bodies, a two-step solvent debinding process, and a continuous thermal debinding-vacuum pressure sintering process, WC-9Co carbide with uniform microstructure, smaller grain size, and relatively uniform distribution were prepared. The Vickers hardness, transverse fracture strength, and fracture toughness were measured to be 1525±3HV30, 3492±45MPa, and 20.4±0.5MPa·m1/2, respectively. The comprehensive mechanical properties were superior to those reported by recent additive manufacturing technologies and comparable to those of WC-Co carbide prepared by traditional powder metallurgy processes.

Main Innovations of the paper of WC-Co carbide additive manufacturing

The use of WC-Co carbide MEX-DS technology to prepare near-full-density WC-9Co carbide, with a transverse fracture strength reaching 3492MPa and a fracture toughness exceeding 20MPa·m1/2, has significantly improved the transverse fracture strength of WC-Co carbide prepared by current AM methods (ranging from 1500-2000 MPa to 3000-4000MPa with HIP treatment) and increased fracture toughness to above 20MPa·m1/2. The comprehensive mechanical properties are significantly better than those reported by similar studies and comparable to similar products prepared by powder metallurgy. The research results are of great significance for addressing the challenging issues of porosity, cracks, and harmful phases encountered in current carbide additive manufacturing and for the development of carbide additive manufacturing technology.

Lascia un commento

Il tuo indirizzo email non sarà pubblicato. I campi obbligatori sono contrassegnati *

日韩亚洲一区二区三区av-欧美综合在线观看一区二区三区| 少妇一区二区三区粉嫩av-国产精品区久久久久久久| 丝袜美腿人妻连续中出-在线观看日韩三级视频| 日韩av电影一区二区网址-老熟妇仑乱视频一区二| 久久久国产精品电影片-精品孕妇人妻一区二区三区| 亚洲欧美激情自拍色图-国产亚洲精品sese在线播放| 亚洲精品激情一区二区-久久成人国产欧美精品一区二区| 国产在线观看高清精品-四季av一区二区三区中文字幕| 亚洲欧美一区二区中文-台湾中文综合网妹子网| 国产在线观看高清精品-四季av一区二区三区中文字幕| 中文不卡一区二区三区-老司机在线老司机在线一区| 色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 久久影视av一区二区-人妻激情乱偷一区二区三区| 国产成人精品免费视频大全办公室-亚洲欧美日本综合在线| 亚洲日本一区二区三区黄色电形-中文字幕乱码免费熟女| 欧美精品一区二区不卡-精品国产一区二区三区香蕉网址| 少妇一区二区三区粉嫩av-国产精品区久久久久久久| 一区二区三区国产高清mm-美女张开腿让帅哥桶爽| 黄片黄片在线免费观看-激情综合网激情五月俺也去| 国产欧美成人精品第一区-日本黄色精品一区二区| 婷婷六月视频在线观看-久久亚洲综合国产精品| 两性污污视频网站在线观看-亚洲欧美日韩激情一区| 婷婷人妻少妇激情在线-欧美日韩人体艺术一区二区| 国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 欧美日韩国产亚洲免费-肉体粗喘娇吟国产91| 亚洲av乱码一区二区-九九免费在线观看视频| 亚洲av专区在线观看国产-丰满人妻av一区二区三区| 欧洲精品一区二区三区中文字幕-91久久国产综合久久蜜月精品| 欧美成人精品巨臀大屁股-亚洲综合欧美日韩一区| 久久精品国产96精品-日韩人成理论午夜福利| 99在线观看精品视频免费-国产极品一区二区三区四区| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 日韩中文字幕v亚洲中文字幕-日韩亚洲av免费在线观看| 三级a级一级大片在线观看-日韩av有码免费观看| 亚洲另类自拍唯美另类-99国产精品兔免久久| 性激烈欧美三级在线播放-久久中文字幕人妻少妇| 日本中文字幕永久在线人妻蜜臀-欧美一区二区的网站在线观看| 亚洲av日韩五月天久热精品-国产日韩欧美一区二区三区群战| 国产精品久久久精品一区-99久久免费精品国产男女性高好|