Binders (also known as forming agents) are critical additives in the powder metallurgy process of cemented carbides. They serve three primary functions during the pressing (forming) stage: enhancing powder flowability, improving binding properties, and increasing green strength. These functions ensure the compact maintains its structural integrity during demolding, handling, and prior to sintering.

Don’t Pick the Wrong Binder?for Your?Cemented Carbide?Production 2
The primary functions of binders in cemented carbide manufacturing

In the powder metallurgy of cemented carbides, binders (also called forming agents) play critical roles, including:

Improving Powder Flowability

Reduces interparticle friction, enabling homogeneous mold filling and uniform compaction.

Prevents powder segregation (e.g., separation of WC and Co).

Enhancing Green Strength

Provides sufficient “green strength” to prevent cracking or edge chipping during handling or demolding.

Minimizes elastic aftereffects (post-compaction expansion).

Lubricating the Mold

Reduces friction between powder and die walls, lowering compaction pressure and extending mold life.

Improves surface finish and minimizes defects (e.g., delamination, cracks).

Facilitating Debinding

Must be fully removable (via thermal decomposition or dissolution) before sintering to avoid carbon residue or impurities that degrade alloy properties.

Performance Requirements for Binders
The binder must possess the following characteristics:

Excellent Compatibility

Uniformly mixes with WC-Co powders without agglomeration or sedimentation.

Chemically inert to powders (e.g., no oxidation of cobalt).

Suitable Melting Point and Viscosity

Melting point must align with compaction temperatures (typically room temperature to 100°C) to ensure:

Liquid-phase homogeneity during mixing.

Solid-phase strength during pressing.

Too high moderate viscosity leads to impedes powder flow.

Too low moderate viscosity leads to insufficient binding force.

High Binding Capacity and Lubricity

Binding capacity: Ensures green strength (flexural strength typically ≥5 MPa).

Lubricity: Reduces compaction pressure (e.g., from 600 MPa to 400 MPa).

Controlled Debinding Behavior

Broad debinding temperature range (e.g., 150–500°C) to prevent cracking from rapid volatilization.

Low carbon residue after debinding (<0.1%) to avoid disrupting alloy carbon balance.

Environmental and Safety Compliance

Non-toxic, low volatility (e.g., water-soluble PEG outperforms solvent-based rubber binders).

Meets industrial emission standards (e.g., sulfur- and chlorine-free).

Cost-Effectiveness

Low-cost and readily available (e.g., paraffin wax is more economical than rubber).

Recyclable or easy to dispose of (e.g., PEG can be water-washed and recovered).

Types of Binder

When manufacturing cemented carbide products, selecting the right binder is crucial for quality and efficiency. Here’s a detailed comparison of the three most common binder types to help you make the best choice for your application.

Paraffin Wax
Don’t Pick the Wrong Binder?for Your?Cemented Carbide?Production 3

Characteristics:Composition: Hydrocarbon-based, solid at room temperature with low melting point (50-70°C)

Best for: Small, simple-shaped carbide products

Advantages:

Excellent lubricity reduces die friction

Low debinding temperature (200-400°C) simplifies processing

Cost-effective and readily available

Limitations:

Lower green strength (prone to cracking)

Potential carbon residue during high-temperature debinding

Temperature-sensitive – requires dry storage

Pro Tip: Ideal for mass production of standard inserts where cost is key.
Don’t Pick the Wrong Binder?for Your?Cemented Carbide?Production 4

PEG (Polyethylene Glycol)

Characteristics:Composition: Water-soluble polymer with adjustable molecular weight (PEG-2000/4000)

Best for: Complex-shaped tools and precision molds

Paraffin wax binder

Advantages:

Higher green strength for intricate shapes

Water-soluble – enables aqueous pre-debinding

Minimal carbon residue

Limitations:

Hygroscopic – requires humidity control

Narrow debinding window (200-300°C)

More expensive than paraffin

Pro Tip: The go-to choice for premium cutting tools requiring precision.

PEG binder

Rubber (SBR, etc.)

Characteristics:Composition: Polymer elastomer requiring organic solvents (e.g., acetone)

Best for: Large, high-density components like rolls and mining tools

Advantages:

Highest green strength

Excellent elasticity prevents cracking

Limitations:

Challenging debinding (500°C+)

Potential sulfur contamination

Environmental concerns with solvents

Highest cost

Pro Tip: Reserved for specialized applications where extreme strength is critical.

Compatibility Principles Between Binders and Wet Milling Media

Paraffin Wax

  • Requires organic solvents (e.g., ethanol, acetone)
  • Limited solubility in ethanol alone – heating often needed

Recommended Medium: Ethanol + 10-20% acetone (enhances solubility)

 

PEG (Polyethylene Glycol)

  • Excellent water solubility
  • Requires oxidation protection for cobalt

Recommended Medium: Deionized water + 0.5% antioxidant (e.g., oxalic acid)

 

Rubber Binders

  • Only soluble in strong organic solvents

Recommended Medium: Pure acetone (requires sealed system to prevent evaporation)

 

Performance Comparison of Three Major Binder Systems

Binding Strength

Rubber binders provide the highest strength due to their polymer chain structure, making them suitable for large compacts. PEG offers moderate strength ideal for complex geometries, while paraffin wax has the lowest binding strength as it relies solely on physical bonding.

Debinding Process

Paraffin wax can be removed at relatively low temperatures between 200 to 400°C, though carbon balance must be carefully controlled. PEG requires aqueous pre-debinding followed by thermal cycling, but is sensitive to moisture. Rubber binders demand high-temperature pyrolysis above 500°C and carry risks of sulfur contamination.

Residue Effects

Paraffin may leave carbon residues that affect the WC/Co ratio, requiring adjustment of carbon potential during sintering. PEG leaves virtually no residue, making it excellent for high-purity alloys. Rubber can leave sulfur residues that reduce the alloy’s corrosion resistance.

Economic Considerations

Paraffin wax has the lowest initial cost but may incur additional expenses for carbon management. PEG provides the best value for precision components and mass production. Rubber is the most expensive option and is only justified for specialized heavy-duty applications.

Selection Summary

For cost-sensitive production where simple processes are preferred, paraffin wax is suitable but requires careful control of dimensional stability during debinding. When high precision and environmental considerations are priorities, PEG is the optimal choice though it needs humidity-controlled storage. Rubber binders are reserved for applications requiring maximum strength and large components, provided that high-temperature debinding equipment is available.

Modern developments are creating hybrid binder systems that combine the advantages of these materials, such as PEG’s performance with paraffin’s cost benefits through advanced formulation techniques.

???????????? ??

???? ???? ??? ???????? ???? ???? ?????. ?????? ?????? ??????? ??? *

欧美一区亚洲一区视频在线观看| 国产精品无码毛片久久久| 加勒比在线不卡一区二区观看| 日本中文字幕无人区一区二区| 色噜噜人妻丝袜中文字幕| 亚洲精品自拍偷拍| 日韩素人精品亚洲热一区| 精品一区二区av天堂色偷偷| 日韩精品高清在线| 亚洲欧美日韩清纯唯美第一区| 狗狗大鸡巴狂操美女| 国产亚洲精品一区久久| 日本入室强伦姧人妻中文| 亚洲卡通动漫第127页| 国产成人精品免费视频全| 骚逼被狂插视频教程| 熟妇女人妻丰满中文字幕| 快速了解国产一级a爱片| 精品久久久久中文字幕人| 老司机精品免费在线视频| 国产亚洲一区二区手机在线观看| 九九视频精品只有这里有| 99亚洲精品高清一二区| 国产一区曰韩二区欧美三区| 最新国产亚洲亚洲精品A| 日韩毛片一区视频免费在线观看| 国产亚洲一区白丝在线观看| 男人的下面进女人的下面在线观看| 97精品人妻人人做人人爽| 999精品免费视频| 精品免费福利片国产| 国产黄片在线免费看| 波多野结衣高潮尿喷| 性一乱一交一免费看视频| 午夜福利在线观看aaa| 国产精品免费第一区二区| 中文字幕无码区一区二区| 高清最新操逼吃鸡巴视频| 国产精品久久久69粉嫩| 国产A级黄片下载| 欧美日韩亚洲人人夜夜澡|