Research status

For WC-Co carbide, the rapidly advancing Powder Bed Fusion (PBF) additive manufacturing (AM) technology has shown unique advantages in producing complex structures of metal parts made of carbide. However, when manufacturing WC-Co carbide with high melting points and high content of hard phases, issues such as difficult-to-eliminate cracks, pores, abnormal grain growth, oxidation decarburization, and brittleness often arise, leading to poor mechanical properties of the produced carbide. In recent years, there have been many reports on the use of Green Additive Manufacturing-Debinding and Sintering (GAM-DS) technology to fabricate WC-Co carbide, which have shown significant advantages in addressing issues such as cracking, abnormal grain growth, oxidation decarburization, and brittleness in PBF carbide. However, the process of preparing green bodies is prone to defects such as pores, interlayer cracks, uneven carbon distribution, and weak local bonding, resulting in problems such as porosity, uneven sintering shrinkage, and uneven microstructure in the sintered bodies. Compared with powder metallurgy, the prepared carbide have relatively low relative densities, and there is a significant gap in mechanical properties.

Brief introduction of research results

Recently, the State Key Laboratory of Powder Metallurgy at Central South University has employed Material Extrusion Additive Manufacturing (MEX) – Debinding and Sintering (DS) technology to successfully produce high-strength and tough WC-9Co cemented carbide with no pores, no cracks, and uniform shrinkage in all directions. Its relative density is approximately 99.7%, and its Vickers hardness, transverse fracture strength, and fracture toughness reach 1525±3HV30, 3492±45MPa, and 20.4±0.5 MPa·m1/2 respectively. The comprehensive mechanical properties are comparable to those of high-performance WC-Co carbide prepared by powder metallurgy processes. The relevant work, titled “Material extrusion additive manufacturing of WC-9Co cemented carbide,” was published in the top international journal “Additive Manufacturing.”

 

research chart

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 2

FIG. 1 Microstructure of MEX WC-9Co cemented carbide green

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 3

FIG. 2 Schematic diagram of stack pore formation of cemented carbide printing green billet: a. MEX stack pore formation; b. Increasing the overlap rate of microfilaments is conducive to reducing the stack porosity of green billet;

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 4

FIG. 3 Microstructure of MEX-DSWC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 5

Figure 4 Micro-CT analysis results of internal defects in MEX-DS WC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 6

Figure 5 Microstructure of WC-9Co cemented carbide: (a) MEX-DS; (b) Press forming – degreasing sintering

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 7

Figure 6 MEX-DS WC-Co carbide Co pool and Co rich zone

WC-Co carbide

Figure 7 Transverse fracture strength and fracture toughness of WC-(8-12)Co cemented carbide prepared by different processes

 

??????

Conclusion of the Paper

(1) By calculating the plasticity index of the printed feedstock with a powder loading of 54 Vol.%, the mechanism of green body printing defects was analyzed, and the green body MEX parameters were optimized. Using optimized parameters such as a printing temperature of 150°C, filament overlap rate of 30%, and printing layer thickness of 0.1mm, defect-free green bodies of WC-9Co cemented carbide with a relative density of 98.5% were prepared.

(2) Both excessively high or low temperatures during the debinding process using n-heptane can lead to debinding cracks. Rapid solvent evaporation during the drying process of debound bodies can also result in microcracks. By employing a two-step solvent debinding process, namely, n-heptane debinding at 30°C for 12 hours followed by kerosene debinding at 30°C for 1 hour, the solvent evaporation rate was reduced, resulting in high-quality debound bodies with no noticeable debinding defects and uniform distribution of binder.

(3) Defects in MEX green bodies can lead to the formation of Co-rich regions or pools, abnormal WC grains, residual pores, etc., in WC-Co carbide. These defects can be improved or eliminated during the sintering process through liquid phase flow and rearrangement of WC particles. By optimizing the MEX green body printing and solvent debinding processes to eliminate printing and debinding defects, it is possible to eliminate defects such as sintering pores, cracks, Co pools, abnormal grain growth, etc., in WC-Co carbide, resulting in near-full-density WC-9Co carbide.

(4) By employing MEX green bodies, a two-step solvent debinding process, and a continuous thermal debinding-vacuum pressure sintering process, WC-9Co carbide with uniform microstructure, smaller grain size, and relatively uniform distribution were prepared. The Vickers hardness, transverse fracture strength, and fracture toughness were measured to be 1525±3HV30, 3492±45MPa, and 20.4±0.5MPa·m1/2, respectively. The comprehensive mechanical properties were superior to those reported by recent additive manufacturing technologies and comparable to those of WC-Co carbide prepared by traditional powder metallurgy processes.

Main Innovations of the paper of WC-Co carbide additive manufacturing

The use of WC-Co carbide MEX-DS technology to prepare near-full-density WC-9Co carbide, with a transverse fracture strength reaching 3492MPa and a fracture toughness exceeding 20MPa·m1/2, has significantly improved the transverse fracture strength of WC-Co carbide prepared by current AM methods (ranging from 1500-2000 MPa to 3000-4000MPa with HIP treatment) and increased fracture toughness to above 20MPa·m1/2. The comprehensive mechanical properties are significantly better than those reported by similar studies and comparable to similar products prepared by powder metallurgy. The research results are of great significance for addressing the challenging issues of porosity, cracks, and harmful phases encountered in current carbide additive manufacturing and for the development of carbide additive manufacturing technology.

???????????? ??

???? ???? ??? ???????? ???? ???? ?????. ?????? ?????? ??????? ??? *

久久99国产综合精品女人-日韩一区二区三区在线不卡| 日本高清二区视频久二区-大香蕉在线视频大香蕉在线视频| 亚洲美女喘息呻吟的网站-国产免费一区二区三区三洲| 久久网站中文字幕精品-三级精品久久中文字幕| 欧美三级韩国三级日本三斤-日本不卡一区不卡二区| 国产精品一区二区欧美视频-国产一区二区三区天码| 中文字幕偷拍亚洲九色-亚洲视频不卡一区二区天堂| 交换朋友的妻子中文字幕-日本美女8x8x8x8| 午夜日韩精品在线视频-亚洲网老鸭窝男人的天堂| 亚洲av乱码一区二区-九九免费在线观看视频| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 97一区二区三区在线-欧美护士性极品hd4k| mm在线精品视频在线观看-欧美国产日韩在线一区二区三区| 7m视频7m精品视频网站-亚洲综合香蕉视频在线| 亚洲国产日韩精品四区-dy888午夜福利精品国产97| av噜噜国产在线观看-欧美视频亚洲视频一区二区三区| 欧美日韩国产综合四区-爆操极品尤物熟妇14p| 日韩av电影一区二区网址-老熟妇仑乱视频一区二| 国内精产熟女自线一二三区-六月丁香婷婷在线观看| av网址在线直接观看-黄色av全部在线观看| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 婷婷六月视频在线观看-久久亚洲综合国产精品| 国产美女裸露无遮挡双奶网站-国产精品色午夜视频免费看| 日韩精品中文在线观看一区-亚洲bt欧美bt精品| 亚洲国产中文欧美一区二区三区-国产精品一区二区视频成人| 18禁真人在线无遮挡羞免费-中文字幕精品一区二区三区四区| 日韩亚洲欧美综合在线-成人在线网站在线观看| 中文字幕社区电影成人-欧美精美视频一区二区三区| 乱入一二三免费在线观看-久久精品亚洲精品国产色婷婷| 亚洲另类熟女国产精品-懂色一区二区三区在线播放| 国语自产偷拍精品视频偷拍-国产伊人这里只有精品视频| 久艹在线观看视频免费-人妻偷人精品一区二区三区| 国产午夜精品理论片A级漫画-久久精品国产99亚洲精品| 一区二区三区日本韩国欧美-日本1区2区3区4区在线观看| 欧美精品一区二区三区爽爽爽-日韩国产精品亚洲经典| 亚洲国产欧美日韩不卡-熟妇激情一区二区三区| 18禁真人在线无遮挡羞免费-中文字幕精品一区二区三区四区| 可以免费看污污视频的网站-日韩欧美不卡视频在线观看| 国产免费高清av在线播放-成年人在线播放中文字幕| 成人免费资源在线观看-欧美国产日韩高清在线综合| 久久久噜噜噜久久狠狠50岁-精品一区二区三区av|