欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

TaC?carbide has been?one of the earliest carbide?put into industrial production?since traditional WC-Co carbides can no longer meet people’s demands for higher product quality. TaC is considered to improve the high-temperature performance of carbide. Meetyou Hardmetal Corp. conducted the following experiment, using WC with different particle sizes as the research object, and studying the properties of TaC tungsten carbide?sintered at different temperatures.

Experiment method

The formulation of the carbide?consists of w(Co)=6.0% and w(TaC)=1.85%. In the WC powder, the mass fraction of particles with an average Fechner size of 4.90μm is 44%, and the mass fraction of particles with a size of 0.89μm is 56%.

The ball-to-powder ratio is 4:1, and the mixture is wet-milled in ethanol at a speed of 50r/min for 65 hours in a 160mm diameter ball mill. Then, the powder is pressed into a B-type bar with dimensions of 20mm x 5.4mm x 6.5mm using a rubber processing procedure. The bars are sintered in a vacuum dewaxing furnace at 1425℃, 1450℃, and 1500℃ for 1.5 hours each.

Afterwards, our experimental staff analyzed the microstructure of the material using scanning electron microscopy, measured its density using an analytical balance, measured its Vickers hardness using a Vickers hardness tester (HV30, with a pressure time of 15 seconds), measured its bending strength using a tensile testing machine, and measured its coercivity using a coercivity meter.

 

Experimental data on TaC carbide

The microstructure of the TaC carbide?material obtained is shown in Figure 1.

sample pic of TaC carbide

From Figure 2, it can be seen that at a sintering temperature of 1425°C, the grain size mainly distributed in ultra-fine grains, showing a normal distribution. At a sintering temperature of 1450°C, the grain size was concentrated in adjacent ultra-fine and ultra-submicron grains, accounting for nearly 70% of the total statistics. The number of nanocrystals also reached its highest value.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 2

At a sintering temperature of 1500°C, the grain size mainly distributed in ultra-fine grains, but some grains grew significantly, resulting in a decrease in the proportion of nanocrystals and ultra-submicron grains, and an increase in the proportion of medium-sized and coarse grains, resulting in a more scattered grain size distribution.

 

Experimental result analysis

The impact of sintering temperature on mechanical properties

The microstructure and properties of the TaC carbide material obtained are shown in Figure 2, where the bending strength and hardness of the sample increase with the increase of sintering temperature. Therefore, when sintered at 1500°C, the TaC carbide grain size continues to grow. From Figure 3, it can be seen that with the increase of sintering temperature, the bending strength value slightly increases.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 3

The bending strength of the carbide?increases as the uniformity of the WC average grain size improves. When the sample is sintered at 1450°C, the average grain size distribution is uniform, and the bending strength slightly increases. When sintered at 1500°C, the excessively high sintering temperature causes the WC grains to grow through the dissolution-precipitation process, and the increase in grain size is beneficial to improve the bending strength of the carbide. However, overall, the change in bending strength value from 914 MPa to 1081 MPa with the increase in temperature is not very significant.

 

 

The effect of sintering temperature on density and coercivity

Figure 4 shows the variation curves of density and coercivity of the samples with the change of sintering temperature. Density is one of the important physical properties of powder metallurgical materials, and the change of compact size during sintering is closely related to the change of density.

Les 3 aspects qui influencent la température de frittage Tac Carbide 4

At 425 ℃ sintering, the shrinkage is incomplete and there are voids present, resulting in a lower density value. With the increase of sintering temperature, the flowability of the bonding phase improves, which is beneficial to eliminate pores and increase the density of the carbide.

When the temperature rises to 1,500 ℃, the volatilization of Co leads to a decrease in the amount of liquid phase, which is not conducive to pore filling, resulting in a decrease in density value.

 

As for coercivity, in WC-Co carbides, the coercivity is mainly related to the Co content and its dispersion. When non-magnetic η-phase appears in the carbide, the coercivity will increase due to the corresponding reduction in the amount of Co phase and the refinement of WC grains. In carbides with normal microstructure, as the carbon content decreases, the tungsten content in the Co phase increases, which strengthens the Co phase and increases the coercivity. At 1450 ℃ sintering, the grains of the sample are refined and evenly distributed, which maximizes the dispersion of the Co phase and thus maximizes the coercivity.

Conclusion

In this study, TaC?carbides were prepared using WC raw materials with different particle sizes and sintered at different temperatures. The following conclusions were drawn:

  1. Under the experimental conditions, the hardness, density, and coercivity of the carbideall first increase and then decrease with the temperature, and the sintering temperature has little effect on the bending strength of the carbide. When sintered at 1450 ℃ and held for 1.5 h, the comprehensive performance of the carbide?is the best, with a Vickers hardness (HV30) of 1668.8, a bending strength of 988 MPa, a density of 14.87 g/cm3, and a coercivity of 15.2 kA/m.
  2. When using mixed particle size WC, TaC has the best inhibitory effect on WC grain at 1450 ℃.

Laisser un commentaire

Votre adresse de messagerie ne sera pas publiée. Les champs obligatoires sont indiqués avec *

99在线观看精品视频免费-国产极品一区二区三区四区| 欧美一级一线在线观看-亚洲一区二区亚洲三区| 97人妻精品一区二区三区爱与-日韩精品亚洲专区在线观看| 中文字幕社区电影成人-欧美精美视频一区二区三区| 美女把腿张开给帅哥桶-无码无套少妇18p在线直播| 欧美日韩国产在线资源-超碰成人国产一区二区三区| 一级小黄片在线免费看-亚洲欧美午夜情伊人888| 91麻豆免费在线视频-欧美中文天堂在线观看| 欧美日韩黑人在线播放-51在线精品免费视频观看| 少妇人妻无码久久久久久-综合图片亚洲网友自拍| 日韩精品一区二区三区粉嫩av-欧美亚洲国产中文字幕| 日韩精品中文在线观看一区-亚洲bt欧美bt精品| 精品国产综合一区二区三区-蜜臀一区二区三区刺激视频| 久久特一级av黄色片-91社区视频免费观看| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 韩漫一区二区在线观看-精品国产免费未成女一区二区三区| 国产免费高清av在线播放-成年人在线播放中文字幕| 日本中文字幕永久在线人妻蜜臀-欧美一区二区的网站在线观看| 亚洲美女喘息呻吟的网站-国产免费一区二区三区三洲| 欧美一级二级三级在线看-日韩精品欧美嫩草久久99| 丝袜美腿人妻连续中出-在线观看日韩三级视频| 精品少妇一区二区18-一区二区三区日韩在线播放| 黄色91av免费在线观看-欧美黄片一级在线观看| 国产精品成人欧美激情-黄色床上完整版高清无遮挡| 亚洲最新国产无人区123-黄片一区二区在线观看| 99在线免费观看视频-丰满人妻一区二区三区视频53| 国产成人精品免费视频大全办公室-亚洲欧美日本综合在线| 日韩精品人妻系列一区-亚洲女同性一区二区三区| 亚洲产国偷v产偷v自拍性色av-亚洲欧美日韩国产三区| 国产成人精品亚洲精品密奴-国产成人AV无码精品| 久久影视av一区二区-人妻激情乱偷一区二区三区| 亚洲最新国产无人区123-黄片一区二区在线观看| 黄色91av免费在线观看-欧美黄片一级在线观看| 欧美亚洲另类久久久精品-国产精品一区二区亚洲推荐| 97人妻精品一区二区三区爱与-日韩精品亚洲专区在线观看| 中文字幕社区电影成人-欧美精美视频一区二区三区| 亚洲黄片三级三级三级-国产成人一区二区在线视频| 久久网站中文字幕精品-三级精品久久中文字幕| 交换朋友的妻子中文字幕-日本美女8x8x8x8| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 国产午夜精品理论片A级漫画-久久精品国产99亚洲精品|