欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

The research and development of crystal plane in cemented carbides is one of the hotspots in the field of cemented carbides both domestically and internationally. The microstructure of the alloy determines its mechanical properties; in WC-Co cemented carbides, the grain size and distribution of the WC phase, as well as the substructure within the grains, are important factors affecting the material’s mechanical properties [10-13]. WC grains have a close-packed hexagonal structure (crystal system P-6m2, a=0.2906nm, c=0.2837nm)24, and the habit planes of WC grains are two basal planes and three prismatic planes. WC grains are prismatic in three-dimensional space, with the basal plane being parallel to the (0001) crystal plane and the prism plane being parallel to the (1-100) crystal plane 5. On the basis of this basic shape, some of the edges and corners are replaced by new crystal planes?6-21. Given that cemented carbides with specific orientations can produce excellent mechanical properties to meet special application requirements, we believe that it is necessary to conduct in-depth research.

This paper takes WC-12Co cemented carbide as the research object. Firstly, nano WC-Co composite powders were prepared by in-situ reduction carbonization reaction at different temperatures, and the composite powders were rapidly densified by discharge plasma sintering technology. The sintered blocks were systematically studied to analyze the effect of the in-situ reduction carbonization reaction temperature on the distribution characteristics of special crystal planes.

Experiment

The raw materials used in the experiment were carbon black, blue tungsten (purity 99.5wt.%, average particle size 50μm) and cobalt oxide (purity 98.5wt.%, average particle size 35μm). Carbon black, blue tungsten, and cobalt oxide were weighed according to the proportion for generating WC-12Co powder, and high-energy ball milling was carried out in a hard alloy ball mill jar with ethanol as the ball milling medium. The mixed powders were subjected to in-situ reduction carbonization reaction at 850°C, 900°C, and 1000°C in a vacuum environment, with a holding time of 1 hour. 2wt% of grain growth inhibitor was added to the composite powders prepared by in-situ reaction, and discharge plasma sintering densification was carried out. The sintering temperature was 1080°C, the holding time was 5 minutes, and the sintering pressure was 60MPa.

Material phase analysis was carried out on a Rigaku D/max-3c X-ray diffractometer with an acceleration voltage of 35kV and a current of 30mA, and a scanning rate of 2°/min. The micro-morphology of the powder was observed on a FEI-NovaNano SEM field emission scanning electron microscope.

Results and of Crystal Plane Distribution

Figure 1 shows the thermogravimetric (TG-DSC) curves of the nano WC-Co composite powder synthesized by in-situ reaction when heated to 1000°C at a heating rate of 10°C/min under Ar gas protection. From the change in the TG curve, it can be seen that as the temperature increases, the mass of the in-situ synthesized WC-Co composite powder decreases. When the temperature reaches 1000°C, the reaction ends, and the powder weight loss reaches nearly 6%. Throughout the heating process, the mass loss of the composite powder is divided into two stages: the first stage is from room temperature to 190°C, where there is a significant decrease in powder mass due to the ease of gas adsorption by nanoscale powders, and the gas desorbs and releases during the heating process, causing powder weight loss; the second stage is from 628°C to 1000°C, where the weight loss rate decreases from high to low. This is because the composite powder did not fully react during the low-temperature in-situ reduction carbonization reaction, and a secondary reaction occurred during the heating process, resulting in rapid weight loss of the powder.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 2

Figure 2 shows the nanoscale WC-Co composite powder prepared by in-situ reduction carbonization reaction at 850°C. The powder particle size is mainly distributed between 30~120nm, with an average particle size of ~83.4nm. The particles have a good sphericity, and spherical or quasi-spherical powders exhibit good dispersibility and flowability, which can effectively avoid hard agglomeration of the powder. This is beneficial for the uniform dispersion of the powder in the sintering mold, thereby ensuring the uniformity and density of the sintered bulk structure. The composite powder prepared by the in-situ reduction carbonization reaction is subjected to rapid sintering densification in an SPS system to obtain nearly fully dense WC-Co cemented carbide blocks. XRD tests are conducted on the alloy specimens in the direction perpendicular to the sintering pressure and in the direction parallel to the sintering pressure. The relative integral intensities (i.e., integral area) of the diffraction peaks for each crystal plane in the VD (vertical to the sintering pressure) and PD (parallel to the sintering pressure) planes of the specimens are obtained through fitting calculations and compared with the relative intensities (integral area) of the diffraction peaks for each crystal plane in the PDF card (which represents the diffraction peak intensity distribution characteristics of traditional sintered cemented carbides), as shown in Table 1. The results indicate that the sintered WC-Co cemented carbide block specimens exhibit a significant characteristic of high anisotropic distribution for specific crystal planes.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 3

Figure 3 shows the XRD patterns of the VD (vertical to the sintering pressure) and PD (parallel to the sintering pressure) planes of the specimens obtained by SPS sintering of the nanoscale WC-Co composite powder prepared by in-situ reaction at 850°C. From the figure, it can be observed that on the PD plane, the intensity of the (0001) plane peak is lower, while the intensity of the (10-10) plane peak is relatively higher. By fitting and calculating the integral area of each diffraction peak, the relative integral area of each crystal plane and the proportion of each crystal plane’s integral area in the total integral area are obtained, as shown in Figures 5 and 6.

 crystal plane distribution
crystal plane distribution

From Figure 5, it can be seen that on the PD plane, the integral area of the (0001) plane accounts for only 10.72% of the total integral area, which is a decrease of 3.3% from the 14.02% in the PDF card (as shown in Figure 4). The proportion of the (10-10) plane reaches 35.73%, which is higher than the 31.87% in the PDF card, and the proportion of the (10-11) plane decreases to 21.76% compared to the 28.11% in the PDF card. Compared to conventional cemented carbide samples, in the PD direction of the composite powder sintered block prepared by in-situ reaction at 850°C, the distribution proportion of the main characteristic planes (0001) and (10-11) decreases, while the distribution proportion of (10-10) increases.

 

Discussion

On the VD direction of the sample, as shown in Figure 6, the proportion of the (0001) crystal plane has significantly increased to 40%, compared to the 14.02% in the PDF card, while the proportion of the (10-10) crystal plane has decreased to 11.68%, a reduction of 20.19% from the 31.87% in the PDF card. From the above analysis, it can be understood that in the sintered block of composite powder prepared by in-situ reaction at 850°C, there is an orientation distribution of characteristic crystal planes. In the direction perpendicular to the pressure, WC grains rotate, causing the (0001) plane to become perpendicular to the pressure direction, thereby reducing the interfacial energy between WC grains. The sintered block of low-temperature in-situ reaction synthesis powder exhibits an orientation distribution characteristic of WC grain characteristic crystal planes, which is believed to be due to the formation of WC grains through secondary reactions during sintering, with atoms preferentially aligning along the (0001) plane and the rotation of WC grains under sintering pressure causing the (0001) plane to tend towards being perpendicular to the pressure direction.

When the temperature is raised to 900°C for in-situ reaction, the prepared composite powder is mainly WC with only a small amount of carbon-deficient phase. When the temperature is raised to 1000°C for in-situ reaction, pure WC-Co composite powder can be obtained. Since the crystal plane distribution of the grains in the powder is isotropic, the crystal plane distribution of WC grains does not change during the subsequent sintering densification process at 900°C and 1000°C, and they still exhibit a randomly distributed isotropic characteristic.

What is the Crystal Plane Distribution of WC-Co Cemented Carbides? 4

Conclusión

1) The nanoscale WC-Co composite powder prepared by low-temperature in-situ reduction carbonization reaction at 850°C can be sintered into cemented carbide block materials with a highly oriented distribution characteristic of WC grain crystal planes using SPS. The sintered blocks of in-situ reaction powder at 900°C and 1000°C maintain an isotropic distribution of WC grain characteristic crystal planes.

2) In the WC-Co cemented carbide with highly oriented characteristic crystal planes, the basal plane (0001) occupies the largest area fraction in the direction perpendicular to the sintering pressure, reaching 40.0%; the prism plane (10-10) occupies the largest area fraction in the direction parallel to the pressure, reaching 35.7%.

3) The phase purity of the composite powder generated by the in-situ reaction plays an important role in the crystal plane orientation of the sintered block. When the main phase of the composite powder is WC, the crystal plane distribution of the sintered block does not exhibit oriented characteristics. However, when the main phase of the composite powder is the carbon-deficient phase, the crystal plane of the sintered block presents an oriented distribution characteristic.

Deja una respuesta

Tu dirección de correo electrónico no será publicada. Los campos obligatorios están marcados con *

国产av剧情护士麻豆-三级国产精品欧美在线观看| 黄片一区二区三区在线看-偷拍一区二区在线观看| 国产老熟女激情小视频-成人一区二区人妻不卡视频| 久久夜色精品亚洲噜国产av-大香蕉伊人猫咪在线观看| 国产人妻人伦精品日本-国产98超碰人人做人人爱| 四虎成人在线免费视频-亚洲熟女中文字幕天堂| 免费看黄色污污的网站-欧美一区二区三区爽爽| 中文字幕精品一区二区日本99-青青国产成人久久91网| 国产黄片在现免费观看-色老板最新在线播放一区二区三区| 少妇人妻无码久久久久久-综合图片亚洲网友自拍| 欧美日本亚一级二级三区久久精品-日韩欧美一区二区久久婷婷| 91精品国产无线乱码在线-999精品视频免费看| 亚洲国产日韩精品四区-dy888午夜福利精品国产97| 亚洲美女喘息呻吟的网站-国产免费一区二区三区三洲| 中文字幕社区电影成人-欧美精美视频一区二区三区| av噜噜国产在线观看-欧美视频亚洲视频一区二区三区| 日韩欧美国产综合久久-国产精品一起草在线观看| 亚洲av乱码一区二区-九九免费在线观看视频| 四虎成人在线免费视频-亚洲熟女中文字幕天堂| av网址在线直接观看-黄色av全部在线观看| 夜夜久久国产精品亚州av-欧美大屁股一区二区三区| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 亚洲av成人一区国产精品网-国产偷_久久一级精品a免费| 18禁真人在线无遮挡羞免费-中文字幕精品一区二区三区四区| 十九禁止观看无码视频-亚洲国产激情福利专区| 精品一区二区三区av在线-欧美黑人巨大精品一区二区| 91亚洲美女视频在线-熟妇人妻精品一区二区三区蜜臀| 亚洲综合久久综合激情-日韩欧美精品人妻二区少妇| 在线观看中午中文乱码-2021国产一级在线观看| 欧美一区二区三区调教视频-三上悠亚国产精品一区二区三区| 熟女少妇免费一区二区-麻豆一区二区三区免费在线观看| 国语自产偷拍精品视频偷拍-国产伊人这里只有精品视频| 人妻日韩精品中文字幕图片-麻豆极度性感诱人在线露脸| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 国产精品久久久精品一区-99久久免费精品国产男女性高好| 国产欧美日本一区二区-一区二区三区亚洲在线播放| 欧美伦乱淫老妇女激情吧-亚洲女邻居精品二区久久| 日韩国产一区二区三区在线-精品日韩人妻少妇av| 亚洲美女喘息呻吟的网站-国产免费一区二区三区三洲| 午夜福利卫生纸福利院-一区二区三区久久亚洲| 亚洲一区二区免费av-中文字幕人妻久久久一区二区三区|