Hyperkarbid = Hyperlegierung + Hartmetall

It is well known that there are two important performance indicators for hard metal alloys: hardness and strength. These two factors are often difficult to balance, much like a seesaw. However, the addition of rhenium to high-temperature alloys can significantly enhance the toughness and high-temperature deformation resistance of materials, including iron-based, nickel-based, and cobalt-based high-temperature alloys.

 

Characteristics of hyper?carbide

hyper?carbide?materials, built upon the foundation of general hard metal alloy constituents, incorporate one or several refractory high-temperature metallic components from hyper?alloys, such as rhenium, ruthenium, osmium, molybdenum, vanadium, tantalum, niobium, etc. This modification imparts exceptional characteristics including higher strength, hardness, and temperature resistance compared to conventional hard metal alloys.

One particularly notable effect is observed when trace amounts of rhenium are introduced into hard metal alloys. This addition significantly enhances and improves the physical properties of hard metal alloy materials, particularly in terms of red hardness and alloy stiffness (elastic modulus). Rhenium applies a solid solution strengthening effect to the existing binding phase metals (iron, cobalt, nickel series) in hard metal alloys, particularly in the realm of high-speed cutting and precision machining of challenging-to-process materials like nickel-based high-temperature alloys, heat-resistant stainless steels, titanium alloys, tungsten-molybdenum-tantalum-niobium-zirconium-hafnium class special alloys. The utilization of cutting tools and precision molds made from these newly developed hyper?carbide?materials presents an extraordinary cost-performance advantage, replacing conventional tools in a remarkable manner.

 

The Principle of Rhenium Enhancement in carbide?Performance

People have come to recognize that adding rhenium to the binder of WC-based hard metal alloys can enhance their high-temperature performance.

Figure 1 schematically depicts the W-Co-Re-C phase diagram under conditions of 9wt% Re + 6wt% Co. This diagram, based on literature and experimental results, is compared with a redrawn phase diagram of WC-Co under conditions of 10wt% Co. Considering that the density of Re is significantly higher than that of Co, the WC-Co-Re hard metal alloy with 9wt% Re and 6wt% Co contains almost the same proportion of binder phase in terms of volume as the WC-Co material with 10wt% Co.

From Figure 1, it is evident that the W-Co-Re-C phase diagram differs from the W-Co-C phase diagram. The following are characteristics of the W-Co-Re-C phase diagram:

Fig1 The W-Co-Re-C phase diagram with 9 wt% Re + 6 wt% Co (red line) compared to the W-Co-C phase diagram with 10 wt% Co (black line).
Fig1 The W-Co-Re-C phase diagram with 9 wt% Re + 6 wt% Co (red line) compared to the W-Co-C phase diagram with 10 wt% Co (black line).

Firstly, in the W-Co-Re-C phase diagram, all melting points shift towards higher temperatures. Therefore, compared to traditional WC-Co materials, WC-Co-Re hard metal alloys require sintering at higher temperatures.

Secondly, for WC-Co-Re hard metal alloys, the two-phase region without the η phase and free carbon slightly shifts towards the higher end at higher carbon contents. This shift is relatively minor but still needs to be considered in the preparation of WC-Co-Re hard metal alloys. It’s worth noting that the width of the two-phase regions in the W-Co-Re-C phase diagram is similar to that in the W-Co-C phase diagram.

Lastly, the addition of rhenium to the binder significantly expands the region where the equilibrium of WC + η phase + liquid phase exists at temperatures above approximately 1430°C. This implies that if medium- to low-carbon and low-carbon content WC-Co-Re hard metal alloys are rapidly cooled from the sintering temperature, they might contain the η phase instead of decomposing into thermodynamically stable WC + Co/Re mixtures. Therefore, post-sintering WC-Co-Re hard metal alloys must be cooled at relatively low cooling rates to ensure complete decomposition of the η phase.

Figure 2 illustrates this, showing that batches of WC-Co-Re with medium to low carbon content contain the encapsulated η phase after rapid cooling, while they don’t contain the η phase after slow cooling.

What is Hyper Carbide? 2
Fig2?Under conditions of cooling from the sintering temperature (1520°C) to 1300°C at different cooling rates: (a – cooling rate of 4°C/minute, b – cooling rate of 0.5°C/minute), the microstructure of a medium-grained WC-Co-Re hard metal alloy with 9wt% Re + 6wt% Co and a total carbon content of 5.45 wt%
Was ist Hyperkarbid? 3
Fig3 Sintered at 1520°C, then slowly cooled to 1250°C, the microstructure of medium-grained WC-10%Co hard metal alloy (left) and medium-grained WC-Co-Re (containing 9wt% Re + 6wt% Co) hard metal alloy (right)

Figures 3 and 4 present the typical microstructures of medium-grained WC-Co-Re hard metal alloy, compared to traditional WC-Co materials prepared from the same level of WC powder. From Figure 3, it is evident that the microstructure of WC-Co-Re hard metal alloy is noticeably finer than that of traditional WC-Co hard metal alloy. Thus, rhenium serves as a potent inhibitor of WC grain growth, restraining the coarsening process of WC. According to research findings, rhenium tends to concentrate at the WC/binder grain boundaries. Therefore, it can be inferred that the role of inhibiting WC grain growth in WC-Co-Re materials is analogous to the inhibitory action of traditional grain growth inhibitors at WC-Co interfaces.

Sub-micron WC-Co-Re hard metal alloys are commonly used in high-temperature and high-pressure components, where the role of rhenium in inhibiting grain growth is crucial. This is significant as it eliminates the need to add conventional grain growth inhibitors to sub-micron WC-Co-Re hard metal alloys. Figures 4 and 5 depict the microstructure of sub-micron WC-Co-Re hard metal alloy without grain growth inhibitors, exhibiting fine and uniform particles without exceptionally large WC grains. The sintering temperature for this hard metal alloy is 1520°C, notably higher than the typical sintering temperature for sub-micron WC-Co alloys.

Was ist Hyperkarbid? 4
Figure 4 shows the microstructures of medium-grained WC-Co-Re hard metal alloy with 9 wt% Re + 6 wt% Co (left) and sub-micron WC-Co-Re hard metal alloy with 5.5 wt% Re + 3.7 wt% Co
What is Hyper Carbide? 5
Figure 5 displays the microstructure of sub-micron WC-Co-Re hard metal alloy with 5.5 wt% Re + 3.7 wt% Co.

 

Performance of hyper?carbide?WC-Co-Re

Research has revealed that WC-Co-Re hard metal alloys exhibit significantly improved physical and mechanical properties at high temperatures. The curves in Figure 6 indicate that the hardness of WC-Co-Re material remains more stable as the temperature decreases (20-800°C) compared to traditional WC-Co hard metal alloys. Operating temperatures of 300°C and 500°C are common for HPHT (High Pressure High Temperature) components. In comparison to conventional WC-Co materials, the hardness of WC-Co-Re hard metal alloy reduces by nearly two times at these two temperatures. Increased thermal hardness is crucial for manufacturing tools used for nickel-based high-temperature alloys or other heat-generating materials. These tools require cutting edges with high thermal stability and mechanical robustness.

Was ist Hyperkarbid? 6

Fig. 6. The hardness variation with temperature when comparing sub-micron WC-Co-Re cemented carbide containing 5. 5 wt % Co + 3. 7 wt % Re with traditional sub-micron cemented carbide containing 6 wt % Co

Figure 6 illustrates the variation of hardness with temperature for sub-micron WC-Co-Re hard metal alloy containing 5.5 wt% Co + 3.7 wt% Re, compared to the traditional sub-micron hard metal alloy with 6 wt% Co.

Based on the previously mentioned higher thermal hardness of WC-Co-Re hard metal alloy, it can be inferred that Re-containing hard metal alloys exhibit improved high-temperature creep resistance. In fact, as depicted in Figure 7, the WC-Co-Re hard metal alloy achieves the same compressive stress rate value under a significantly higher load than conventional WC-Co material. This suggests that the Co-Re binder demonstrates significantly enhanced high-temperature creep performance.

Was ist Hyperkarbid? 7

Figure 7 illustrates the relationship between strain rate and compressive stress for WC-Co-Re and WC-Co hard metal alloys at 800°C.

Schreibe einen Kommentar

Deine E-Mail-Adresse wird nicht ver?ffentlicht. Erforderliche Felder sind mit * markiert.

国产人妻人伦精品日本-国产98超碰人人做人人爱| 亚洲欧美精品在线一区-99热国产在线手机精品99| 四虎成人在线免费视频-亚洲熟女中文字幕天堂| 日韩毛片在线免费人视频-超碰中文字幕av在线| 99久久精品一区二区成人-麻豆国产av玩弄放荡人妇系列| 黄色91av免费在线观看-欧美黄片一级在线观看| 欧美日韩亚洲1区2区-黄污视频在线观看不卡| 麻豆久久国产精品亚洲-日本理论中文字幕在线视频| 久色高清精品在线国产-国产精品视频一区三区四区| 亚洲日本一区二区三区黄色电形-中文字幕乱码免费熟女| 欧洲精品一区二区三区中文字幕-91久久国产综合久久蜜月精品| 黄片黄片在线免费观看-激情综合网激情五月俺也去| 国产精品久久99精品毛片-国产四季高清一区二区三区| 黄片一区二区三区在线看-偷拍一区二区在线观看| 国产精品一区二区欧美视频-国产一区二区三区天码| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 人妻少妇无乱码中文字幕-人成免费视频一区二区| 欧美日韩国产综合四区-爆操极品尤物熟妇14p| 少妇人妻无码久久久久久-综合图片亚洲网友自拍| 国产精品电影在线一区-亚洲国产大片一区二区官网| av一区免费在线观看-中文字幕日韩国产精品视频| 欧美aa一级视频播放-久一一区二区三区大香蕉| av中文字幕男人天堂-懂色av一区二区三区在线观看| 欧美亚洲另类久久久精品-国产精品一区二区亚洲推荐| 午夜福利1区2区3区-午夜洗澡免费视频网站| 亚洲国产欧美日韩不卡-熟妇激情一区二区三区| 国产一区二区无套内射-国内精品久久久久久久齐pp| av一区免费在线观看-中文字幕日韩国产精品视频| 天天日天天干天天综合-99久久综合狠狠综合久久| 日本少妇激情一区二区-亚洲自偷自拍熟女另类蜜臀| 青青操视频在线观看国产-欧美成人乱码在线观看| 国产欧美日韩精品一区在线-久久精品视频免费获取地址| av网址在线直接观看-黄色av全部在线观看| 可以免费看污污视频的网站-日韩欧美不卡视频在线观看| 久久99热这里都是精品啊-国产成人亚洲精品无码aV| 精彩亚洲一区二区三区-中文字幕中文字幕在线色站| 午夜福利1区2区3区-午夜洗澡免费视频网站| 深夜三级福利在线播放-日韩精品一区二区在线天天狠天| 国产精品久久久精品一区-99久久免费精品国产男女性高好| 十九禁止观看无码视频-亚洲国产激情福利专区| 一区二区三区女同性恋-熟妇高潮一区二区高清网络视频|