Why should we study nanoceramic bonded carbide? As we all know, WC-Co carbide consists of hard phase (WC) and bonding phase (ferrous metal). In harsh environments, the bonding phase is more susceptible to corrosion and oxidation than the hard phase, which limits its application in some fields. Therefore, reducing the content of the bonding phase is considered to solve this problem. In addition, metal Co is an expensive material and has a certain impact on human health. It is necessary to reduce the application of Co in carbide from the perspective of reducing costs and human health.

Nanoceramic bonded phase WC-based carbide refers to a type of carbide product that does not contain or contains a small amount of metal bonding agent (<0.5% by mass fraction). It has unparalleled excellent wear resistance, corrosion resistance, excellent polishing, and oxidation resistance compared to traditional carbide.

nanoceramic bonded phase WC-based carbide is a combination of ceramic hardness and carbide toughness, and products have been launched abroad. With its excellent wear and corrosion resistance, it can be used to make sandblasting nozzles, electronic packaging materials, heavy-duty sliding seal wear-resistant parts, etc.. with its excellent cutting performance, it can be used as tool and drill materials, especially for processing titanium/titanium alloys, which greatly improves work efficiency. and with its oxidation resistance and excellent polishing, it can be used as mold and decorative materials.

nanoceramic bonded carbide's micro structure

Characteristics of nanoceramic bonded carbide:

1Phase structure and carbon content of nanoceramic bonded phase carbide carbide are very sensitive to carbon content. For traditional carbide containing bonding phases, there is a certain range of carbon content to maintain a normal phase structure. If this range is exceeded, brittle n-phase or free carbon will appear. In contrast, the suitable carbon content of nanoceramic bonded phase WC-based carbide is not fluctuating like WC-Co alloy but is a fixed value.

2Composition design and properties of nanoceramic bonded carbide

Nanoceramic bonded carbide, which combine mechanical and wear resistance properties perfectly, are one of the most widely used ceramic-based materials in engineering. However, in most ceramic-based materials, the existence of metal bonding phases not only makes these composite materials have excellent flexural toughness but also affects certain properties, which limits their use. In addition, the low melting point of metal Co also greatly limits the application of WC-Co cutting tools in high-speed machining, which is prone to serious adhesive wear and oxidation wear. Moreover, the poor corrosion resistance, high cost, and toxicity of Co also limit the mechanical industry application of WC-Co carbide. Therefore, partially or completely replacing the Co bonding phase can expand the application of carbide. In recent years, ceramic bonding phases have attracted widespread attention in the scientific community as a new type of Co substitute.

 

The specific study using Nanoceramics as Binder Phase in Hardmetal Alloys

The Research Institute of Shandong University in China selected nanoscale Al2O3, ZrO2, and MgO as the binder phase for WC hardmetal alloys. The microstructure and mechanical properties of the hardmetal alloys were compared, and the toughening mechanism of the nanoceramic oxides was explored. The related paper, titled “Nano-ceramic replacing cobalt in cemented carbide as binder phase: Is it feasible?”, was published in the Journal of Alloys and Compounds.

Paper link:

https://linkinghub.elsevier.com/retrieve/pii/S0925838821043784

 

What is nanoceramic bonded carbide? 1

 

 

 

 

4Mechanism of Ceramic Binders Improving Toughness of carbide?Materials

What is nanoceramic bonded carbide? 2

fig.1 TEM micrographs of nanoceramic bonded carbide: (a) dislocations in WC-6Al2O3, (b) dislocations in WC-6ZrO2, (c) dislocations in WC-6MgO, and (d) intragranular and intergranular microstructures of WC-6ZrO2.

After sintering, the WC grains retained their initial grain size, and the second phase significantly suppressed the grain growth of the WC matrix by limiting grain boundary migration. Dislocations were observed in all three nanoceramic bonded carbide materials, which enhanced the tolerance of the carbide. Additionally, it was found that some nanoscale ZrO2 grains were distributed along the WC grain boundaries, while more ZrO2 nanograins were distributed within the WC grains, forming so-called intragranular nanostructures. Compared with the ceramic binder phase at the WC grain boundaries, the ceramics inside the WC grains were smaller in size.

What is nanoceramic bonded carbide? 3

fig.2 The toughening mechanism of WC-6Al2O3

What is nanoceramic bonded carbide? 4

fig.3 The toughening mechanism of WC-6ZrO2

What is nanoceramic bonded carbide? 5

fig.4 The toughening mechanism of WC-6AMgO

During the high-temperature sintering and cooling process, residual tensile stresses are generated around the ceramic binder phase due to differences in thermal expansion coefficient, which is favorable for crack deflection when the crack reaches the stress field. When an external load is applied to the nano-ceramic binder material, the difference in elastic modulus causes a redistribution of microscopic stress, thereby increasing the material’s toughness. All three nanoceramic bonded carbide materials exhibit crack bridging, effectively reducing crack propagation energy. Non-branching cracks were also found in the carbide, greatly increasing the energy consumption of the main crack propagation and effectively slowing down crack propagation.

What is nanoceramic bonded carbide? 6

fig.5 XRD spectra of the polished surface and fractured surface of the WC-6ZrO2 specimen

During the fracture process of WC-ZrO2 carbide, when external stress is applied to the carbide, stress concentration occurs near the crack tip, promoting the transformation of t-ZrO2 to monoclinic m-ZrO2. This transformation significantly impedes the crack propagation by enhancing stress relaxation near the crack tip. In addition, the volume expansion caused by phase transformation compresses the surrounding matrix, which is conducive to crack closure. Furthermore, surface phase transformation can generate compressive stress, greatly increasing the toughness of the material.

???????

In summary, compared with traditional WC-Co carbide, nanoceramic bonded carbide exhibit a better combination of fracture toughness and hardness. Compared with micro-ceramic bonded? carbide, the hardness and fracture toughness of nano-ceramic bonded phase carbide are simultaneously enhanced. This excellent hardness of nano-ceramic bonded phase carbide is crucial for high-speed machining applications and is expected to become a candidate material for high-speed machining tools.

???? ???????

?? ??? ??? ????? ????? ??????????. ?????? ????????? ???? ????? ?? *

日韩二级视频在线观看-美女扒开奶罩露出奶子的视频网站| 日韩毛片在线免费人视频-超碰中文字幕av在线| av一区免费在线观看-中文字幕日韩国产精品视频| 国产成人精品免费视频大全办公室-亚洲欧美日本综合在线| 久久蜜桃精品一区二区-麻豆视频啊啊啊好舒服| 久久99热这里都是精品啊-国产成人亚洲精品无码aV| 国产精品中出久久久蜜臀-久久久中国精品视频久久久| 久久高清超碰av热热久久-国产高清不卡免费视频| 人妻互换精品一区二区-夜夜爽一区二区三区视频| 日韩精品人妻系列一区-亚洲女同性一区二区三区| 婷婷人妻少妇激情在线-欧美日韩人体艺术一区二区| 蜜臀一区二区三区精品在线-99久久久精品免费看国产| 91麻豆免费在线视频-欧美中文天堂在线观看| 国产成人精品亚洲精品密奴-国产成人AV无码精品| 黄色av网站在线免费观看-亚洲欧美精品偷拍tv| 久久精品亚洲国产av久-国产精品视频一区二区免费| 精品老熟妇一区二区三区-日韩丰满一区二区三区| 91精品国产无线乱码在线-999精品视频免费看| 欧美精品一区二区不卡-精品国产一区二区三区香蕉网址| 日本欧美在线视频观看-国产一区二区三区无码下载快播| 久久蜜桃精品一区二区-麻豆视频啊啊啊好舒服| 青青操视频在线观看国产-欧美成人乱码在线观看| 91亚洲美女视频在线-熟妇人妻精品一区二区三区蜜臀| 亚洲欧美日韩国产一区二区三区-国产欧美日韩一区二区免费| 久久亚州天堂一区二区-色噜噜色哟哟一区二区三区| 久久人妻一区二区三区欧美-国内不卡的一区二区三区| 黄色91av免费在线观看-欧美黄片一级在线观看| 亚洲午夜久久久精品影院-性感美女在线观看网站国产| 午夜日韩精品在线视频-亚洲网老鸭窝男人的天堂| 欧美精品一区二区三区爽爽爽-日韩国产精品亚洲经典| 国产老熟女激情小视频-成人一区二区人妻不卡视频| 亚洲女人黄色录像一区-日韩av电影在线免费看| 麻豆久久国产精品亚洲-日本理论中文字幕在线视频| 久久久国产精品电影片-精品孕妇人妻一区二区三区| 五月婷婷六月在线观看视频-亚洲黑寡妇黄色一级片| 色婷婷六月婷婷一区二区-91草草国产欧美在线观看| 国产精品美女在线网址-久草免费福利在线观看视频| 国内精产熟女自线一二三区-六月丁香婷婷在线观看| 97人妻精品一区二区三区爱与-日韩精品亚洲专区在线观看| 国产美女网站在线观看-国产精品亚洲综合网69| 蜜臀一区二区三区精品在线-99久久久精品免费看国产|