欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

The size of WC grains is of great significance to the friction and wear properties of cemented carbide. It is generally believed that coarse-grained cemented carbide has poorer wear resistance than fine-grained cemented carbide. After the grain refinement of cemented carbide, the size of the hard phase decreases, increasing the surface area of the hard phase grains and the bonding force between the grains, and the binder phase is more evenly distributed around them, which can improve the hardness and wear resistance of the cemented carbide. In this paper, the author conducts friction and wear experiments on cemented carbide to analyze the friction and wear properties under different parameters and the material removal mechanism, providing experimental evidence for the optimization design of high-speed cutting tool materials, reasonable material selection, and the study of high-speed cutting wear mechanisms.

Experiment

Test Materials

Three types of WC-6Co cemented carbide with different grain sizes were selected for the test. The size of the cemented carbide disc was φ55mm×4mm, and the surface was rough ground, finely ground, and polished. The mating material used was Al?O? balls with a diameter of 9.5mm. Both samples were ultrasonically cleaned in acetone for 20 minutes and dried for use. The material properties are shown in Table 1.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 2

Friction and Wear Test

The test was conducted on a UMT-2 multi-functional friction and wear testing machine produced by CETR Corporation in the United States, using a ball-on-disc contact method. The structure of the testing machine is shown in Figure 1. The cemented carbide friction disc was attached to the working table with double-sided tape, and the Al?O? ball was placed in the fixture. The two types of mating materials produced mutual movement and force of action. The friction force generated was detected by the sensor, and the curves of friction force, normal force, and friction coefficient were automatically generated by the related software according to Coulomb’s law.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 3

The test was conducted at room temperature, with normal forces of 10N and 20N respectively, and the linear velocities of the friction pair sliding were 40m/min, 80m/min, 120m/min, and 160m/min. The sliding distance was 500m. After the test, a scanning electron microscope (SEM) was used to observe the wear scar surface morphology of the upper and lower samples, and an X-ray energy dispersive spectrometer (EDS) was used to detect the elemental composition of the worn surfaces. All samples were analyzed for the elemental composition of the friction and wear surfaces under the same conditions.

Results and Analysis

Friction and Wear Performance

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 4

Figure 2 shows the friction coefficient curve of ZH cemented carbide drawn by the testing machine’s accompanying software (load 20N, sliding speed 160m/min). The experiment found that each friction process follows a similar pattern, that is, the initial dynamic friction coefficient undergoes a rapid increase from the initial value during the transition period, and then remains relatively stable, showing a fluctuating characteristic in the stable phase. In the beginning, under the action of the normal load, only local micro-convex bodies on the friction surface are in contact, the adhesive area is small, and the molecular attraction on the contact surface is weak, so the friction coefficient is small; as the friction process progresses, the micro-convex bodies interfere with each other, gradually get worn down, the adhesive area increases, and the molecular attraction also increases, leading to a gradual increase in the friction coefficient. The entire friction process is a continuous process of the contact surface adhering and then being sheared under the action of shear stress. Due to the peeling and breaking of the Co phase on the surface, the wear of the sample surface occurs, and the local adhesion on the surface quickly reaches a dynamic equilibrium, resulting in the friction coefficient of the surface being maintained within a relatively stable range, which is called the stable period.

Most scholars use the average value of the friction coefficient over a period of time (distance) as a characterization parameter of friction behavior. Therefore, this experiment selects the average value during the stable friction phase as the friction coefficient of the cemented carbide under the corresponding parameters. Figure 3 shows the friction coefficients of three types of cemented carbide under different loads and speeds.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 5

It can be seen that with the increase of friction speed and load, the friction coefficient of the cemented carbide generally shows a decreasing trend, and the decrease is most obvious in the transition from relatively low speed (40m/min and 80m/min) to high speed (120m/min and 160m/min). From the perspective of material, the friction coefficient of ZH cemented carbide is smaller than that of the other two materials, and the friction coefficients of ZHX and HG cemented carbides are not significantly different, with the friction coefficient of HG cemented carbide being slightly larger.

Wear Mechanism

After the friction and wear tests, the microstructure of the worn surfaces of each sample was observed using a scanning electron microscope (SEM), and SEM images were taken, along with an analysis of the surface composition. The friction and wear mechanisms of the cemented carbide under different friction parameters are similar, as shown in Figure 4 (sliding speed 160m/min, load 20N).

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 6

In the initial stage of cemented carbide wear, the binder phase Co undergoes plastic deformation, and the surface layer of Co is extruded by the WC grains. Due to the low hardness and good ductility of Co, under certain conditions, a micron-scale friction film can form on the surface, while the harder WC particles gradually protrude from the friction surface, preventing further rapid wear of the surface and allowing the friction process to enter a relatively stable stage. As the binder phase Co continues to be lost, the WC framework of the material is damaged, and the dislocation density within the WC particles significantly increases. When the dislocation density accumulates to a certain extent, microcracks will form on the WC particles, causing the WC particles to begin to pull out from the cemented carbide matrix. The detached WC particles remain in the wear area, transforming into abrasive particles, which, under the action of the load, compress against the matrix, resulting in new plastic deformation and grain damage.

cemented carbide

As can be seen from Figure 4, as the grain size of the cemented carbide decreases, the grain density increases, and the degree of surface wear decreases. The surface of the ZHX cemented carbide shows no obvious shedding of WC particles, while the surface density of HG is very good, with almost no obvious shedding of WC particles. Therefore, for the traditional grain size cemented carbide ZH, the main wear mechanism is abrasive wear caused by the extrusion of the binder phase Co and the shedding of WC grains. As the grain size decreases and the density of the fine-grained cemented carbide increases, the phenomenon of WC grain spalling decreases, Co still wraps around the WC, the microstructure of the material remains intact, and most grains only undergo a certain degree of plastic deformation.

???????

The size of WC grains has an important effect on the friction and wear properties of cemented carbide. As the grain size decreases, the friction coefficient slightly increases, and the wear resistance is enhanced.

The friction coefficient of cemented carbide is influenced by speed and load, and it shows a decreasing trend with the increase of speed and load.

The wear mechanism of traditional grain size cemented carbide is mainly characterized by the extrusion of the binder phase Co and the fracture and spalling of the hard phase WC grains; the grain spalling phenomenon of fine-grained cemented carbide is not obvious, and the main wear mechanism is plastic deformation.

???? ???????

?? ??? ??? ????? ????? ??????????. ?????? ????????? ???? ????? ?? *

亚洲欧美精品中文字幕乱码-欧美丰满肥臀大屁股熟妇激情-97人妻精品一区二区三区久久久-亚洲国产永久精品成人麻豆| 免费亚洲成人av在线播放-日本av一区二区三区四区-久久久精品人妻一区二区三区色秀-雪白大屁股在线观看视频| 亚洲欧美国产日韩在线-少妇被粗大的猛烈进出免费-色综合天天狠天天狼天天透天-av免费在线播放一区二区| 伊人精彩视频在线免费观看-欧洲精品码一区二区三区免费看-97黄色成人在线网站-国产av无遮挡屁股喷水| 色哟哟精品一区二区三区四区-精品人妻一区二区三区蜜桃九-婷婷久久亚洲中文字幕-国产久久热这里只有精品| 人妻少妇精品性色av免费-国产精品自拍av一区二区-亚洲欧美国产另类91综合-在线观看国产高清自拍| 亚洲综合一区二区国产精品-西西日本极品丰满少妇-美女激情性感午夜小视频-丰满人妻中文字幕乱码一区二区| 99久久婷婷精品国产综合-色婷婷六月激情久久综合-av福利导福航大全在线播放-97久久一精品人妻人人玩| 亚洲国产av一区二区三区伊在-欧美日韩精品人妻二区三区-午夜精品一区二区三区可下载-最新国产精品视频久久久| 亚洲制服丝袜欧美另类-日韩女优在线一区二区三区-国产伦久视频免费观看视频-少妇挑战三个黑人还被内射| 91精品国产成人一区二区-白丝老师好紧好爽好湿作文-国产成人久久流白浆图-丰满少妇猛烈进出高清晰视频| 人妻一区二区三区四区免费-在线亚洲国产网红av-国产成人精品免费视频小-中老年熟妇激情啪啪大屁股| 一区二区在线观看少妇高潮-欧美午夜不卡在线观看免费-人妻精品一区二区三区在线-少妇又紧又深又湿又爽视频紫| 伊人精彩视频在线免费观看-欧洲精品码一区二区三区免费看-97黄色成人在线网站-国产av无遮挡屁股喷水| 97精品人妻一区二区三区麻豆-亚洲最大av在线观看网址-欧美日韩精品一区二区三区不卡-亚洲熟伦熟女新五十路熟女| 久久久婷婷成人就要色成人-亚洲中出视频在线观看-亚洲精品中文字幕有码-免费男女做爰免费视频| 国产av熟女一区二区三区四区-尤物国产精品福利在线网-91亚洲国产成人久久精品-97色伦在线视频播放| 狠狠躁夜夜躁人人爽野战天天-91密桃精品国产91久久-欧美亚洲另类久久综合-亚洲精品中文字幕视频在线| 亚洲中文高清在线观看-久久久国产精品亚洲专区91-中文字幕免费一区二区三区乱码-国产成人精品国内自产拍在线| 91免费精品国自产拍偷拍-亚洲中文字幕av一区二区三区-av男人的天堂在线免费观看-青草视频在线播放免费| 性a一级在线视频免费观看-国产一级一片内射视频播放蘑菇-99精品视频看国产啪视频-日韩欧美一线本在线播放| 精品久久久人妻中文免费-综合激情久久狠狠伊人五月-av在线男人的免费天堂-中文字幕av一区人妻少妇| 国内av一区二区三区在线看-国产精品亚洲一区二区三区久久-欧产日产国产精品不卡-97人妻精品一区二区三区在线| 欧美亚洲国产精品日韩-亚洲黄色片成年人免费观看-人摸人人人澡人人超碰av-亚洲一区二区中文字幕在线观看| 女厕偷窥一区二区三区在线-五月婷婷伊人中文字幕-一个人免费完整视频高清-中文字幕人妻在线一区二区三区| 人妻一区二区三区久久丰满-久久天天躁夜夜躁狠狠综合-久久久精品中文字幕免费-亚洲av盗摄不卡在线| 亚洲一级一片内射在线播放-精品人妻中文字幕一区二区三区-精品国产最大网站麻豆-嫩草伊人久久精品少妇蜜桃av| 91亚洲一线产区二线产区-亚洲国产精品不卡一二-亚洲视频在线中文字幕国产区视频-人妻熟女一区二区在线观看| 成人看的毛片美女高潮自-精品中文字幕一区二区三区av-欧美国产亚洲自拍第二页-国产成人精品性色av麻豆| 国产av精品一区二区三区久久-隔壁的日本人妻中文字幕版-日韩精品福利一区二区三区-邻居人妻少妇好紧好爽呀中| 国产精品亚洲欧美日韩久久-深夜av免费在线观看-亚洲熟妇中文字幕五十中出-国产精品一区二区成人久久| 中文字幕最新有码在线-91亚洲国产一区二区三区-国内精品伊人久久久av高清-国产成人精品午夜在线播放| 亚洲国产av一区二区三区伊在-欧美日韩精品人妻二区三区-午夜精品一区二区三区可下载-最新国产精品视频久久久| 国产一区二区三区av福利-日本人妻乱交中文字幕-欧美日韩欧美在线免费观看-疯狂放荡的少妇免费观看| 亚洲无人区乱码中文字幕首页-亚洲欧美国产日韩丝袜美腿-国产久久精品一区二区亚洲-疯狂进入丝袜人妻一区二区| 久久久久久久久国产精品-粗大挺进尤物人妻身体的视频-国产成人精品播放在线-久久亚洲av午夜福利精品一区| 亚洲制服丝袜欧美另类-日韩女优在线一区二区三区-国产伦久视频免费观看视频-少妇挑战三个黑人还被内射| 国产艳妇av在线观看果冻传媒-97人妻精品一区二区免费-国产成人三级一区二区在线观看-日韩av大片一区二区三区| 精品久久人人妻人人澡人人爽-五月激情开心久久婷婷-久久国内精品一区二区三区-有码中文字幕一区二区三区| 久久精品国产96精品亚洲-中文字幕有码视频在线观看-日本黄色激情按摩作爱啪啪视频-欧美激情欧美啪欧美视频| 亚洲国产精品一区二区三区色-白嫩肥妇一区二区三区av-久久精品国产亚洲av高清-风韵犹存丰满大屁股熟女国产|