欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

Based on the different hard phases, corrosion-resistant cemented carbides can currently be classified into three major categories: WC-based, Cr?C?-based, and TiC-based, with WC-based cemented carbides occupying the largest proportion. Therefore, it is necessary to study the corrosion resistance of this type of alloy. This paper investigates the corrosion resistance of WC-based cemented carbides in acids and alkalis, as well as its relationship with the content and composition of the binder phase, graphite, and η1 phase in the alloy. On this basis, the activated sintering of cemented carbides with low binder phase content is also explored.

Introduction to the Corrosion Resistance of Tungsten Carbides 2

Sample Preparation and Experimental Conditions

Material Selection

To compare the corrosion resistance of WC-based cemented carbides, four groups of test materials were selected:
(1) WC-Co alloy;
(2) WC-Co alloy with a small amount of heterogeneous carbides;
(3) WC-Ni·Mo·Co·Cr alloy;
(4) Low binder phase content alloy.

Corrosion Conditions

Corrosion Media: Hydrochloric acid, sulfuric acid, nitric acid, citric acid (H?Cit), acetic acid (HAC), sodium hydroxide (50%), and potassium hydroxide (50%).
Test Temperatures: 20°C, 40°C, 80°C, and boiling point. Alkali solutions were only tested at the boiling point.
Corrosion Time: 24-72 hours for low temperatures and 6-24 hours for the boiling point.
Corrosion Rate Calculation: The corrosion rate (A) is calculated as the amount of material corroded per unit area per day, expressed in mg/dm2·day (abbreviated as mdd).

Introduction to the Corrosion Resistance of Tungsten Carbides 3

Results and Discussion

Relationship Between Corrosion Rate and Binder Phase Content in WC-Based Cemented Carbides

The corrosion rate of WC-based cemented carbides is related to the content of the binder phase, regardless of the binder’s composition. Alloys with higher binder content exhibit higher corrosion rates. For WC-Co alloys, when the cobalt content exceeds 2%, the corrosion rate increases sharply. In 5% HNO?, the corrosion rate of WC-2% Co alloy still exceeds the acceptable limit. However, the corrosion rate of WC-Ni·Mo·Co·Cr alloy with 2% Ni·Mo·Co·Cr meets the usage requirements under all tested conditions. Even in highly corrosive nitric acid, its corrosion rate is only 196.6 mdd, corresponding to corrosion resistance grade B (less than 250 mdd).

The difference in corrosion rates among alloys with varying cobalt content is not significant at room temperature. However, as the temperature increases, the difference becomes more pronounced. At room temperature, increasing the cobalt content from 2% to 20% results in a corrosion rate change of only 12-30 mdd. At the boiling point, the corrosion rate increases from 20 mdd for low cobalt content to 6×10? mdd for high cobalt content.

Effect of WC Grain Size on Corrosion Rate

Fine-grained alloys have higher interfacial energy and greater internal stress in the binder phase, resulting in lower corrosion resistance. Therefore, fine-grained alloys are not recommended for improving resistance.

Effect of Small Amounts of Heterogeneous Carbides on Corrosion Rate

Comparing WC-Co cemented carbides with small amounts of heterogeneous carbides reveals that their effects on corrosion rates vary:

Cr?C?: A small amount of Cr?C? can improve the alloy’s corrosion resistance. Even though alloy No. 9 has finer WC grains than alloy No. 4, its corrosion resistance is superior due to the addition of Cr?C?.

TaC: The addition of a small amount of TaC has no significant effect on resistance. Comparing alloy No. 4 with alloy No. 7 (which contains 2% TaC), the corrosion rates are similar. Adding 5% TaC also does not improve corrosion resistance.

Mo?C: Adding less than 1% Mo?C can significantly enhance resistance. This is because Mo?C readily dissolves in the γ phase, thereby improving the alloy’s corrosion resistance.

Thus, adding small amounts of Cr?C? or Mo?C is beneficial for improving the corrosion resistance of cemented carbides.

Effect of Graphite and η1 Phase on Alloy Corrosion Rate

The presence of graphite and η1 phase not only significantly affects the physical and mechanical properties of the alloy but also has a notable impact on the corrosion rate. For the tested media, the presence of graphite significantly reduces the alloy’s corrosion resistance. When graphite is present, the solubility of tungsten (or molybdenum) in the binder phase drops below 2-3%, reducing the binder phase’s resistance. Additionally, according to corrosion theory, graphite increases the electrochemical corrosion effect of micro-galvanic cells between phases. Therefore, cemented carbides used as corrosion-resistant materials must avoid the formation of graphite.

In contrast, the η1 phase significantly enhances the alloy’s corrosion resistance. The presence of η1 phase indicates carbon deficiency in the alloy, allowing the binder phase to dissolve a large amount of W (or Mo), typically 10-13%. This composition of the binder phase is more corrosion-resistant. Moreover, the transformation of a certain amount of binder into η1 phase further improves the alloy’s resistance. Thus, under carbon-deficient conditions, the alloy’s corrosion resistance increases sharply compared to normal alloys.

Given these findings, the carbon content should be controlled at the lower limit of the two-phase region or allow the formation of a small amount of dispersed η1 phase, provided that the mechanical properties are not excessively compromised. This results in an ideal microstructure with high corrosion resistance.

Relationship Between Binder Phase Corrosion Resistance and Alloy Corrosion Rate

While the mechanical properties of WC-Ni alloys are generally lower than those of WC-Co alloys, their corrosion resistance is superior, especially under low-carbon conditions. However, alloys with pure nickel as the binder often fail to meet usage requirements, leading to the development of complex nickel-based binders. Ni-Mo alloys exhibit excellent resistance to acid and alkali corrosion, making them suitable as binders for WC-based alloys. This study tested the corrosion resistance of alloys with Ni-Mo-Co-Cr (83:15:1:1) as the binder. The overall trend in corrosion rates for this series is similar to that of WC-Co alloys, but the values are significantly lower. Particularly, low binder content alloys meet the specified usage requirements for all tested media, with corrosion rates below 250 mdd. Additionally, the corrosion rate of WC-Ni·Mo·Co·Cr alloys does not change significantly with increasing temperature.

In summary, improving the corrosion resistance of WC-based cemented carbides depends on enhancing the binder phase’s corrosion resistance, which is particularly effective for low binder content alloys.

Activated Sintering of WC-Based Low Binder Content Alloys

An important approach to improving the resistance of WC-based cemented carbides is to reduce the binder content, provided that the physical and mechanical properties meet usage requirements.

To enhance the performance of sintered products, activated sintering is often employed. The properties of low binder content alloys are closely related to the uniformity of component mixing. Therefore, chemical mixing to produce composite powders, intensified ball milling, and activated sintering processes were adopted. For comparison, conventional processes were also used to prepare alloys with the same composition.

Comparison of Corrosion Resistance Among Different Alloys

Corrosion rates are classified into three grades: A (<25 mdd), B (<250 mdd), and C (<500 mdd). For WC-Co alloys, only low binder content alloys exhibit comprehensive corrosion resistance. In contrast, WC-Ni·Mo·Co·Cr alloys maintain considerable corrosion resistance even with 10% binder content. Notably, WC-2% Ni·Mo·Co·Cr alloys demonstrate excellent resistance under all tested conditions.

WC-Ni·Mo·Co·Cr alloys are widely used in manufacturing ballpoint pen tips. These alloys outperform traditional WC-Co·Ni·Cr alloys in various properties, are easier to produce, and have lower production costs, making them ideal materials for corrosion-resistant ballpoint pen tips.

corrosion resistance

Conclusions

1.The corrosion resistance of WC-based cemented carbides is primarily determined by the resistance of the binder phase. Lower binder content results in better condition. Alloys with Ni·Mo·Co·Cr as the binder exhibit significantly lower corrosion rates than WC-Co alloys, especially those with low binder content.

2.The corrosion rate of WC-based cemented carbides is related to the grain size of the hard phase. Finer grains lead to poorer corrosion resistance.

3.Small amounts of heterogeneous carbides, such as Cr?C? and Mo?C, can improve the resistance of WC-Co alloys, while TaC has little to no effect.

4.Graphite reduces the resistance of WC-based alloys, whereas the η1 phase significantly enhances it. Therefore, the ideal corrosion-resistant alloy should have carbon content controlled at the lower limit of the two-phase region or allow the formation of dispersed η1 phase without excessively compromising mechanical properties.

5.Low binder content alloys with good corrosion resistance can be prepared using chemical mixing to produce composite powders, intensified ball milling, and activated sintering processes, achieving high physical and mechanical properties.

6.The study of the corrosion resistance of WC-based cemented carbides provides a basis for their broader application.

???? ???????

?? ??? ??? ????? ????? ??????????. ?????? ????????? ???? ????? ?? *

日本女优一卡二卡在线观看-欧美大胆a级视频秒播| 亚洲综合av一区二区三区-高潮又爽又黄无遮挡激情视频| 久久网址一区二区精品视频-日产国产欧美视频一区精品| 国产欧美日本一区二区-一区二区三区亚洲在线播放| 国产免费一区二区三区不-日本少妇免费一区二区三区| 婷婷六月视频在线观看-久久亚洲综合国产精品| 国产精品久久99精品毛片-国产四季高清一区二区三区| 人妻日韩精品中文字幕图片-麻豆极度性感诱人在线露脸| 国产精品电影在线一区-亚洲国产大片一区二区官网| 黄片免费观看视频下载-国产丝袜诱惑在线视频| 成人免费资源在线观看-欧美国产日韩高清在线综合| 青木玲高清中文字幕在线看-视频在线免费观看你懂的| 在线免费观看黄片喷水-国产精品白丝网站在线观看| 亚洲欧美日韩二区三区-国产在线欧美一区日韩二区| 在线观看中午中文乱码-2021国产一级在线观看| 黄片黄片在线免费观看-激情综合网激情五月俺也去| 小12萝自慰喷水亚洲网站-chinese偷拍一区二区三区| 久久精品亚洲国产av久-国产精品视频一区二区免费| 亚洲福利视频免费观看-中文字幕日本不卡一区二区| 国产在线观看高清精品-四季av一区二区三区中文字幕| 欧美日韩精品人妻在线-在线播放中文字幕一区| 欧美日韩国产综合新一区-国产综合av一区二区三区| 精品老熟妇一区二区三区-日韩丰满一区二区三区| 麻豆久久国产精品亚洲-日本理论中文字幕在线视频| hd在线观看一区二区-免费一区二区三区毛片在线| 亚洲区欧美区在线视频-亚洲碰碰人人AV熟女天堂| 欧美视频在线观看国产专区-亚洲91精品在线观看| 国产aa视频一区二区三区-国产精品久久久久久久毛片动漫| 亚洲女人黄色录像一区-日韩av电影在线免费看| 免费av一区在线观看-国产精品视频高潮流白浆视频免费| sobo欧美在线视频-免费av网址一区二区| 国内精产熟女自线一二三区-六月丁香婷婷在线观看| 日韩精品一区二区三区十八-日韩人妻少妇一区二区三区| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 91精品国产无线乱码在线-999精品视频免费看| 亚洲愉拍自拍欧美精品app-亚洲一区不卡在线视频| 男女做爰猛烈啪啪吃奶在线观看-人妻连裤丝袜中文字幕| 亚洲一区二区免费av-中文字幕人妻久久久一区二区三区| 人妻互换精品一区二区-夜夜爽一区二区三区视频| 免费看黄色污污的网站-欧美一区二区三区爽爽| 欧美日韩亚洲1区2区-黄污视频在线观看不卡|