In recent years, the production technology of ultra-fine grain cemented carbide has developed rapidly, especially in the key technology of preparing ultra-fine grain WC powder, where the competition is very fierce. Many promising methods have emerged, some of which have reached the level of practical application. However, there are few reports in domestic literature, especially on basic theories or regularity research. In the process of developing the preparation technology of ultra-fine grain WC powder, this paper deeply investigates the influence of the particle size of carbon black powder on the carbon content of WC powder under different carbonization temperatures when using ultra-fine (0.35 μm) tungsten powder.

 

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 2

Experimental Content and Method

Test Materials of WC powder

(1) Ultra-fine tungsten powder: The ultra-fine tungsten powder is prepared by the ultrasonic spray pyrolysis method from ultra-fine WO? powder, which is generally amorphous with an average particle size of 25~30 nm. It is reduced by hydrogen at a medium temperature (750~780℃) to obtain tungsten powder with an average particle size of ≤0.35μm (BET particle size).

(2) Carbon black powder: Carbon black powder is produced by two methods: one is by cracking ethane and propane (at 850℃) and then subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.1 and 0.3 μm, respectively; the other is from activated carbon powder with an original particle size of 100~200μm, which is subjected to high-energy ball milling for different periods to produce carbon black powders with average particle sizes of 0.8 and 4.5 μm, respectively.

Experimental Method

Using ultra-fine tungsten powder with the same particle size (0.35 μm) and four different particle sizes (0.1, 0.3, 0.8, 4.5 μm) of carbon black powder, the carbon is blended according to the reaction formula W+C=WC (with an additional loss of 0.1%). The mixture is ball milled for 1.5 hours in a conventional ball mill with a ball-to-material ratio of 1:1. The heat-resistant stainless steel boat containing the mixed material is placed in a stainless steel tube furnace and carbonized under a hydrogen atmosphere. The holding time is 40 minutes for all. In the temperature range of 830~1300℃, the carbonized material is taken out at different temperatures, cooled, and then removed from the furnace. Subsequently, XRD phase analysis and chemical analysis are conducted to determine the total carbon and free carbon, and the amount of combined carbon in WC is calculated. Finally, the quantitative relationship between the particle size of carbon black powder and the phase composition and combined carbon content of WC powder under different carbonization temperatures can be plotted.

 

Test Results and Discussion

Figure 1 shows the effect of carbon black powder with different particle sizes carbonized at different temperatures on the combined carbon content of WC powder. Curve 1 in Figure 1 represents the relationship between carbonization temperature and the combined carbon content of WC powder when using ultra-fine carbon black powder with a particle size of 0.1 μm. As can be seen from Figure 1, when using 0.1 μm ultra-fine carbon black, the combined carbon content of WC powder can reach 5.8% (by mass), which is equivalent to 95% of the theoretical content, at a very low carbonization temperature (850℃). When the temperature is greater than 950℃, the carbon content of WC powder can reach the theoretical content. This result indicates that the carbonization reaction can be completed at a low temperature when using ultra-fine tungsten powder in conjunction with ultra-fine carbon black powder. This phenomenon suggests that the ultra-fine W powder particles are carbonized before they undergo significant aggregation and growth.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 3
At this temperature, as the particle size of the carbon black used increases, the combined carbon content in WC powder rapidly decreases. For example, as shown in Curve 2 of Figure 1, when using 0.3 μm carbon black at 950℃ with the same holding time of 40 minutes, the combined carbon content of WC powder only reaches 5.2% (by mass). XRD analysis indicates that there is still significant W?C in the WC powder, as shown in Figure 2. The free carbon phase was not detected due to its low content. The combined carbon content in WC powder can only reach the theoretical value when the temperature is increased to 1060℃. Its complete carbonization temperature is about 130℃ higher than that of the 0.1 μm carbon black.

The Influence of Carbon Black Particle Size on the Carbon Content of WC Powder 4

When using 0.8 μm carbon black, as shown in Curve 3 of Figure 1, at 950℃ with a holding time of 40 minutes, the combined carbon content of WC is only 3.18% (by mass). XRD analysis indicates that in addition to the obvious W?C phase, there is also significant free carbon present in the WC powder, as shown in Figure 3. The combined carbon content in WC powder can only reach the theoretical value when the carbonization temperature is increased to 1230℃. The temperature required for complete carbonization has increased significantly.
The reason for this phenomenon is that when the carbon content ratio is constant, the finer the carbon black particle size, the easier it is to mix uniformly with W powder particles, increasing the contact area between them. Undoubtedly, fine-grained carbon black will accelerate the carbonization rate. Moreover, the finer the carbon black particle size, the more its specific surface area and the number of active carbon atoms on the surface increase dramatically. Thus, the carbonization reaction rate between carbon and tungsten accelerates, and the complete carbonization temperature decreases with the decrease of carbon black particle size.

WC powder

Conclusions

(1) When the particle size of ultra-fine W powder is the same (≤0.35μm), the combined carbon content in WC powder decreases significantly with the increase of the carbon black particle size at a certain temperature.
(2) When the particle size of carbon black is constant, the content of combined carbon increases with the rise of carbonization temperature.

Leave a Reply

Your email address will not be published. Required fields are marked *

免费看黄色污污的网站-欧美一区二区三区爽爽| 欧美看片一区二区三区-人妻无卡精品视频在线| 欧洲精品一区二区三区中文字幕-91久久国产综合久久蜜月精品| 久久99热这里都是精品啊-国产成人亚洲精品无码aV| 日本中文字幕啊啊啊啊-久久精品伊人久久精品伊人| 亚洲国产精品一区二区av-日本一级黄色一区二区| 99在线观看精品视频免费-国产极品一区二区三区四区| 欧美字幕一区二区三区-好吊妞欧美一区二区在线观看| 少妇人妻无码久久久久久-综合图片亚洲网友自拍| 狠狠狠狠爱精品一二三四区-l舌熟女av国产精品| 成人av一区二区蜜桃-亚洲色图激情人妻欧美| 91麻豆免费在线视频-欧美中文天堂在线观看| 久久精品国产亚洲av湖南-竹菊精品一区二区三区| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 久久网站中文字幕精品-三级精品久久中文字幕| 国产精品二区高清在线-91精品91久久久久久| 十九禁止观看无码视频-亚洲国产激情福利专区| 99在线观看精品视频免费-国产极品一区二区三区四区| 国产成人高清精品免费5388-好妞色妞在线视频播放| 97香蕉久久国产在线观看-麻豆黄色广告免费看片| 精品少妇一区二区18-一区二区三区日韩在线播放| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 在线免费观看黄片喷水-国产精品白丝网站在线观看| 亚洲福利视频免费观看-中文字幕日本不卡一区二区| 国产av剧情护士麻豆-三级国产精品欧美在线观看| 国产精品一区二区欧美视频-国产一区二区三区天码| 国产在线不卡高清一区-日本一区二区三区四区无卡| 久久99热这里都是精品啊-国产成人亚洲精品无码aV| 欧美一级一线在线观看-亚洲一区二区亚洲三区| 欧美日韩成人在线观看-久久五月婷婷免费视频| 亚洲精品激情一区二区-久久成人国产欧美精品一区二区| 在线观看中午中文乱码-2021国产一级在线观看| 久久蜜桃精品一区二区-麻豆视频啊啊啊好舒服| 日韩亚洲一区二区三区av-欧美综合在线观看一区二区三区| 免费av一区在线观看-国产精品视频高潮流白浆视频免费| 亚洲女人黄色录像一区-日韩av电影在线免费看| 久久久噜噜噜久久狠狠50岁-精品一区二区三区av| 欧美日韩国产亚洲免费-肉体粗喘娇吟国产91| 国产一级片久久免费看同-麻豆精品尤物一区二区青青| 青青操大香蕉在线播放-国产亚洲欧美精品在线观看| 深夜三级福利在线播放-日韩精品一区二区在线天天狠天|